Group: Forum Members
Posts: 688,
Visits: 5.4K
|
Looks like bridging from the pictures. You haven't got the cloth into the recesses in the mould. Because pre-preg is quite resin light there isn't enough resin to fill the voids. With infusion the voids would have filled with resin, still not ideal but you wouldn't have those dry spots. You really need to force the cloth into any recesses/tight corners to ensure it is in full contact with the mould surface. With pre-preg being sticky it won,t move in the mould even when you pull vac.
Warren
Carbon Copies Ltd
|