Warren (Staff)
Warren (Staff)
Supreme Being (33K reputation)Supreme Being (33K reputation)Supreme Being (33K reputation)Supreme Being (33K reputation)Supreme Being (33K reputation)Supreme Being (33K reputation)Supreme Being (33K reputation)Supreme Being (33K reputation)Supreme Being (33K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
That is a much better finish.  As said, corner bridging can make a real difference. So pay special attention to the corners.  Also you can try holding it at the soak temperature for a bit longer to see if that helps resin flow.  

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
KLComposites
KLComposites
Supreme Being (309 reputation)Supreme Being (309 reputation)Supreme Being (309 reputation)Supreme Being (309 reputation)Supreme Being (309 reputation)Supreme Being (309 reputation)Supreme Being (309 reputation)Supreme Being (309 reputation)Supreme Being (309 reputation)
Group: Forum Members
Posts: 26, Visits: 3.2K
Any bridging in the corners will draw resin away from the field and lead to pinholes. Not much resin to go around. Also, if you use peel ply, especially on thin laminates, you'll draw too much resin out of the part. 
carguy84
c
Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)
Group: Forum Members
Posts: 6, Visits: 176
So I took more care in doing the vacuum bagging and making sure there wasn't any leaks in the bag or the tubing and it came out MUCH better, but still am getting pin holes:

https://imgur.com/a/wCN3t4G
But it's a 1000 times better than the first run.



carguy84
c
Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)
Group: Forum Members
Posts: 6, Visits: 176
until my ramp and soak controller ships I'm a little behind the curve for temp processing, but Omega says it should ship this week.  In the mean time I am going to check the bag and do a drop test spending a lot of time going over everything.  thanks!
Lester Populaire
L
Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)
Group: Forum Members
Posts: 311, Visits: 13K
carguy84 - 1/4/2021 12:41:10 PM
I did a debulk after the first layer but I did not have the breather go all the way up the sides of the mold, I can try that today.  After looking around the internet some more, I'm thinking I may have had a leak in the bag somewhere, will be on the lookout for that as well.  Other than that I have no idea.

Out of autoclave prepreg can be quite unforgiving in terms of process parameters...

carguy84
c
Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)
Group: Forum Members
Posts: 6, Visits: 176
I did a debulk after the first layer but I did not have the breather go all the way up the sides of the mold, I can try that today.  After looking around the internet some more, I'm thinking I may have had a leak in the bag somewhere, will be on the lookout for that as well.  Other than that I have no idea.
Lester Populaire
L
Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)
Group: Forum Members
Posts: 311, Visits: 13K
carguy84 - 1/4/2021 12:47:04 AM
Not sure what went wrong with this. It’s two ply of the XC110 on an EB700 board that’s been CNCd, sanded and sealed with 120. EB700 machines excellent, BTW.

I used FibRelease on the surface of the mold and cured it in the curing oven with the ramp to 70c, hold for 4 hours, ramp to 120 and held that for about 80 minutes and then let it cool in the oven back down to 25. I don’t have a ramp and soak controller yet, just a regular Auberins one, but did my best to manually follow the ramp up in the doc.

The part came right out of the mold but with the surface seen here. Seems like a lot of the resin ended up on the back side of the part. Too much vacuum isn't a thing right?  You can run the vacuum the entire time?  Does this look more like bad bagging technique?  My stack is bagging, cloth on the bottom and under the hose adapter and then just the release over the carbon.

Thanks for any advice.

Chip-

https://imgur.com/a/0djWj9T


I would say use a breather on the whole circumference and debulk after the first layer.

carguy84
c
Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)Forum Guru (74 reputation)
Group: Forum Members
Posts: 6, Visits: 176
Not sure what went wrong with this. It’s two ply of the XC110 on an EB700 board that’s been CNCd, sanded and sealed with 120. EB700 machines excellent, BTW.

I used FibRelease on the surface of the mold and cured it in the curing oven with the ramp to 70c, hold for 4 hours, ramp to 120 and held that for about 80 minutes and then let it cool in the oven back down to 25. I don’t have a ramp and soak controller yet, just a regular Auberins one, but did my best to manually follow the ramp up in the doc.

The part came right out of the mold but with the surface seen here. Seems like a lot of the resin ended up on the back side of the part. Too much vacuum isn't a thing right?  You can run the vacuum the entire time?  Does this look more like bad bagging technique?  My stack is bagging, cloth on the bottom and under the hose adapter and then just the release over the carbon.

Thanks for any advice.

Chip-

https://imgur.com/a/0djWj9T


Edited 5 Years Ago by carguy84
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search