If its not coming out the mould, assuming release agent applied correctly, then it probably needs a bit more time to cure. Part cured or green resins tend to grip the mould and can be hard to demould.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
ana
a
ana
posted 6 Years Ago HOT
Supreme Being (256 reputation)Supreme Being (256 reputation)Supreme Being (256 reputation)Supreme Being (256 reputation)Supreme Being (256 reputation)Supreme Being (256 reputation)Supreme Being (256 reputation)Supreme Being (256 reputation)Supreme Being (256 reputation)
Group: Forum Members
Posts: 14, Visits: 49
Warren (Staff) - 10/12/2020 12:13:06 PM
Sometimes with variation in thickness you need to allow more time to ensure an even cure throughout otherwise you can get issues where subsequent resin layers react with the gel causing delamination or surface shrink back and aligatoring type effects.  Most gels will have a sufficient open time for double gelling or layup against to allow sufficient cure time and getting the backing layer on safely. 

Tanks so much Warren for your advise
Also please help me

I apply gel coat as first layer . After 2 hrs I apply second layer " mixed polyester resin around 35% and 5 % pigment and silica powder 30 % and carbonate calcium 30 % as filler 
I demold after 1 hrs but back side of mold comes out very good but top side is not come out easily ." Gel coat side "
Please help me what is my problem ?
Also I add cobalt 0.05 % " 10 % "and peroxide 1.8 %
How can i remove my part easily ?
My part thickness is 1.2 mm

Edited 6 Years Ago by ana
Warren (Staff)
Warren (Staff)
Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Sometimes with variation in thickness you need to allow more time to ensure an even cure throughout otherwise you can get issues where subsequent resin layers react with the gel causing delamination or surface shrink back and aligatoring type effects.  Most gels will have a sufficient open time for double gelling or layup against to allow sufficient cure time and getting the backing layer on safely. 

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
ana
a
ana
posted 6 Years Ago HOT
Supreme Being (256 reputation)Supreme Being (256 reputation)Supreme Being (256 reputation)Supreme Being (256 reputation)Supreme Being (256 reputation)Supreme Being (256 reputation)Supreme Being (256 reputation)Supreme Being (256 reputation)Supreme Being (256 reputation)
Group: Forum Members
Posts: 14, Visits: 49
hi
please help me

I apply gel coat on the mold (
cast mold )
. but some area I applied more gel coat and these area  is thicker than another area ( some area has  mm gel coat and some area has 1.3mm gel coat. is it possible to different thickness effects on the
de-molding of my part from mold?
if yes, please let me know what is it exactly?

2- if i add more cobalt to polyester resin what is the effect of de-molding the part? is good or is not good?

tanks so much
Edited 6 Years Ago by ana
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search