Carbon brakes have absolutely nothing to do with usual carbon composites, from a process view. As a hobbyist you will not get the materials or the equipment.
The process I was involved in was this: resin impregnated fibres (not epoxy) were placed into a mould and baked. This burned the resin, leaving only graphite.  after this the now porous material was infused with resin and baked several times to get rid of the porosity.  So in the end you get a carbon fibre reinforced graphite material, which is much more heat resistant than any crp.
So no, it is absolutely not a straight forward process.

Steve Broad
Steve Broad
Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)
Group: Forum Members
Posts: 408, Visits: 4.1K
scottracing - 4/20/2020 8:37:05 PM
f1rob - 4/20/2020 7:57:41 PM
Carbon brakes are "grown"
They start with basic carbon cloth "web"
Burn the correct gasses at the right pressure and the right temperature  ( VERY HOT ) and  slowly pure carbon particles form.
Takes about 6 weeks to grow a disc.
Modern discs have slightly diffrent characteristics as they alter the gasses used an the various quantities 
Originally the discs that were used in f1 were the off cuts from the plane industry.
F1 discs were the centres that were cut out off the discs for Boeing 747


Pretty much what rob says. I thought they took more than 6 weeks and more like 3 months. 
But I certainly wouldn't look into trying to make some.
I bought a couple to make into light fitting bases and they were relatively cheap.

Yeah, I guess it problematic post curing the discs to 1000 dec C :-)

f1rob
f1rob
Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)
Group: Forum Members
Posts: 237, Visits: 4.8K
scottracing - 4/20/2020 8:37:05 PM
f1rob - 4/20/2020 7:57:41 PM
Carbon brakes are "grown"
They start with basic carbon cloth "web"
Burn the correct gasses at the right pressure and the right temperature  ( VERY HOT ) and  slowly pure carbon particles form.
Takes about 6 weeks to grow a disc.
Modern discs have slightly diffrent characteristics as they alter the gasses used an the various quantities 
Originally the discs that were used in f1 were the off cuts from the plane industry.
F1 discs were the centres that were cut out off the discs for Boeing 747


Pretty much what rob says. I thought they took more than 6 weeks and more like 3 months. 
But I certainly wouldn't look into trying to make some.
I bought a couple to make into light fitting bases and they were relatively cheap.

Hi mate rumour has it the boys at ks tried to make discs with high temp pre preg
Didn't end well surprisingly 

scottracing
scottracing
Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)
Group: Forum Members
Posts: 460, Visits: 5.2K
f1rob - 4/20/2020 7:57:41 PM
Carbon brakes are "grown"
They start with basic carbon cloth "web"
Burn the correct gasses at the right pressure and the right temperature  ( VERY HOT ) and  slowly pure carbon particles form.
Takes about 6 weeks to grow a disc.
Modern discs have slightly diffrent characteristics as they alter the gasses used an the various quantities 
Originally the discs that were used in f1 were the off cuts from the plane industry.
F1 discs were the centres that were cut out off the discs for Boeing 747


Pretty much what rob says. I thought they took more than 6 weeks and more like 3 months. 
But I certainly wouldn't look into trying to make some.
I bought a couple to make into light fitting bases and they were relatively cheap.

f1rob
f1rob
Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)
Group: Forum Members
Posts: 237, Visits: 4.8K
Carbon brakes are "grown"
They start with basic carbon cloth "web"
Burn the correct gasses at the right pressure and the right temperature  ( VERY HOT ) and  slowly pure carbon particles form.
Takes about 6 weeks to grow a disc.
Modern discs have slightly diffrent characteristics as they alter the gasses used an the various quantities 
Originally the discs that were used in f1 were the off cuts from the plane industry.
F1 discs were the centres that were cut out off the discs for Boeing 747


k.alan.bates
k
Supreme Being (348 reputation)Supreme Being (348 reputation)Supreme Being (348 reputation)Supreme Being (348 reputation)Supreme Being (348 reputation)Supreme Being (348 reputation)Supreme Being (348 reputation)Supreme Being (348 reputation)Supreme Being (348 reputation)
Group: Forum Members
Posts: 36, Visits: 664
Has anyone succeeded in making their own carbon fiber brake rotors and bads for a carbon on carbon braking system for a race car?

...What kind of process did you follow for making them?
Any special considerations?
How did you test them?

I'm just curious to know if it would be as straightforward as it seems it would be or if there is some "secret magic" that prevents mere mortals from attempting the feat.

Thanks

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search