Post curing a tool for prepreg after pulled off it's tool?


Author
Message
Hanaldo
Hanaldo
Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Yeh it was a big disappointment for me as Duratec is my go-to pattern coating. The XT135 definitely needs to be cured in contact with epoxy though, it just pinholes badly against any polyester or vinylester surface. It's just much easier to wet-lay an epoxy tool and get a perfect surface finish off the Duratec, so I've virtually given up on the XT135 - even though it's such a joyful way to make moulds 😔
scottracing
scottracing
Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)
Group: Forum Members
Posts: 460, Visits: 5.2K
handy to know tooling preg and duratec dont mix, ive not had the joy of mixing the two together! 


quinn
q
Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)
Group: Forum Members
Posts: 155, Visits: 992
Hanaldo - 1/21/2019 10:28:53 PM
Tooling pre-preg doesnt like Duratec, I have tested that myself and don't recommend trying it.

There is no problem at all with post-curing a mould off the plug, the trick is to do it extremely slowly. If you can do any sort of elevated temp cure on the plug then this definitely helps, even if it is only 40C; 80C is even better. Once off the plug, you need a very controlled ramp rate of 0.1° per minute, with soaks every 10° for at least a couple of hours. Remember that print through is a product of low resin content, so a resin infused CF sheet is very likely to suffer a lot of print through. A wet-lay mould with a surface coat should see less print-through, but you also want to maintain dimensional accuracy, so a slow ramp rate is very important.

Excellent, sounds good. I'll do a low heat cure on the plug. Even though the duratec could handle 80c, the mdf might expand a bit and put hairline cracks in the duratec so I'll probably just do 40 or 50c if that's enough to help, then very carefully post cure off the plug. Makes sense now why my infused panel had print through from post curing. I'll make sure to get a nice coating of surface coat on the plug so there's no weave near the surface. I'll have to do some testing to get my oven to ramp slow enough. Should slow way down with a single bulb, maybe even get a lower wattage bulb. 

Hanaldo
Hanaldo
Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Tooling pre-preg doesnt like Duratec, I have tested that myself and don't recommend trying it.

There is no problem at all with post-curing a mould off the plug, the trick is to do it extremely slowly. If you can do any sort of elevated temp cure on the plug then this definitely helps, even if it is only 40C; 80C is even better. Once off the plug, you need a very controlled ramp rate of 0.1° per minute, with soaks every 10° for at least a couple of hours. Remember that print through is a product of low resin content, so a resin infused CF sheet is very likely to suffer a lot of print through. A wet-lay mould with a surface coat should see less print-through, but you also want to maintain dimensional accuracy, so a slow ramp rate is very important.
scottracing
scottracing
Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)Supreme Being (6.1K reputation)
Group: Forum Members
Posts: 460, Visits: 5.2K
have you considered using tooling prepreg? It cures at 50-60 degrees then post cures up to 180 degrees.


quinn
q
Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)
Group: Forum Members
Posts: 155, Visits: 992
So I'm switching to prepreg for my helicopter canopies. Need to make a female mold that can handle 120c. Because of how the plug is made, the mold can't be made with prepreg. I mill my plug out of mdf, spray with duratec surface primer, then sand/polish. The duratec is only specd to handle about 95c so that's why I can't bake a prepreg mold on it.  I ordered some room temp cure high temp tooling epoxy and high temp surface coat. Plan is to brush the high temp surface coat onto the plug  (after frekote is applied) then do carbon fiber wet lay on top of that to create the mold. I will let it cure at room temp, then remove it from the plug and post cure the mold in the oven. Will this work? Or is it an issue to post cure a mold after it's been removed from the plug? Reason I ask is, I once post cured a cf sheet that had a perfect glossy surface. During the post cure, the surface finish got much worse. Had visible print through and lost it's nice gloss. Is this gonna happen to my mold if post curing after removing it from the plug? I could at least post cure on the plug up to 80c or so if that helps, then remove it from the plug and cure the rest of the way. Thoughts?