Group: Forum Members
Posts: 592,
Visits: 1.9K
|
I assume what you mean is that you get the infusion mesh printing through the peelply?
Just use an extra layer of peelply under the infusion mesh ..It will use a bit more (wasted) resin, but should stop print-through from the infusion mesh.
I get all sorts of "print" on the reverse side of my infusions, from the creases in the peelply, creases and folds in the vacuum bag, but usually they are removed with the peelply.
If i want a good finish on the reverse side i usually use two layers of peel ply and sand it down, then coat with epoxy or clearcoat.
"Sapere Aude"... Dare to KNOW!
The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...
103% of all people do not understand statistics...
Do not adjust our mind, theres a fault in reality :-)
|