Infused a flat panel for the 1st part of my dash, and have got some small slit like marks in the resin.

Unfortunately they don't show up when I photograph them - very small little slits, 5mm long max, and about the width of a letter l.

I'm thinking I didn't shut off resin long enough before the vacuum perhaps ? and they are air bubbles ?

Any ideas ?
Hanaldo
Hanaldo
Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)Supreme Being (32K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Definitely sounds like voids, but more likely caused by being a little on the lean side. Try clamping the vacuum line, then let the resin flow into the part for another 20-30 seconds. 
MarkMK
MarkMK
Supreme Being (4.3K reputation)Supreme Being (4.3K reputation)Supreme Being (4.3K reputation)Supreme Being (4.3K reputation)Supreme Being (4.3K reputation)Supreme Being (4.3K reputation)Supreme Being (4.3K reputation)Supreme Being (4.3K reputation)Supreme Being (4.3K reputation)
Group: Forum Members
Posts: 338, Visits: 2K
As Hanaldo said, it does sound like voids

Make sure you entire stack of materials has wetted through prior to clamping-off the resin feed, even if it means a little resin finding it's way into the catch pot.
fgayford
fgayford
Supreme Being (5.9K reputation)Supreme Being (5.9K reputation)Supreme Being (5.9K reputation)Supreme Being (5.9K reputation)Supreme Being (5.9K reputation)Supreme Being (5.9K reputation)Supreme Being (5.9K reputation)Supreme Being (5.9K reputation)Supreme Being (5.9K reputation)
Group: Forum Members
Posts: 433, Visits: 1.2K
Davo456 (04/04/2016)
Infused a flat panel for the 1st part of my dash, and have got some small slit like marks in the resin.

Unfortunately they don't show up when I photograph them - very small little slits, 5mm long max, and about the width of a letter l.

I'm thinking I didn't shut off resin long enough before the vacuum perhaps ? and they are air bubbles ?

Any ideas ?


I agree with the quotes below. I will add this to the mix. Always make sure your mold is warm to the touch before you infuse, not just room temperature. I place my molds in my over and get them warm before I infuse and it makes a big difference in reducing pinholes. I also heat my resin as well. This advice is from experience and not a try this and lets see what happens sort of thing.
Hope this helps you out.
Fred

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search