111mattin111 (09/02/2016)
OK so came out of the mould all nicely but for the first time I've had print through from the soric can see the honeycomb through the carbon? http://www.talkcomposites.com/Uploads/Images/01a40327-2e3c-4124-b046-3f3e.jpg


Cores will always print. Soric has less print, but they do always print. It's caused by the larger quantities of resin in the channels of the core shrinking more. When it is cold (I'm assuming you are in Europe), the resin takes longer to cure, so when you demould after 24 hours it won't be quite fully cured and it will print sooner. You can reduce it slightly by leaving the part to cure longer in the mould, but it will eventually print. Post-coating helps reduce the appearance of it. 
Matthieu Libeert
Matthieu Libeert
Supreme Being (10K reputation)Supreme Being (10K reputation)Supreme Being (10K reputation)Supreme Being (10K reputation)Supreme Being (10K reputation)Supreme Being (10K reputation)Supreme Being (10K reputation)Supreme Being (10K reputation)Supreme Being (10K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
just give it a few tabs like you would launch marbles with you fingers like from back in the days and it should go down all the way then Wink If full vacuum ofcourse! 

Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




111mattin111
111mattin111
Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)
Group: Forum Members
Posts: 67, Visits: 910
OK so came out of the mould all nicely but for the first time I've had print through from the soric can see the honeycomb through the carbon? http://www.talkcomposites.com/Uploads/Images/01a40327-2e3c-4124-b046-3f3e.jpg
111mattin111
111mattin111
Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)
Group: Forum Members
Posts: 67, Visits: 910
Thanks for that Matt
The parts infused now all went nicely so will demould later 
And see how it turns out 👍
Matt (Staff)
Matt (Staff)
Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)
Group: Forum Members
Posts: 680, Visits: 1.9K

Hi Mattin,

Definitely doesn't look like something to worry about here: these are notscientifically calibrated gauges and should be used as a guide not a precisioninstrument.

Atmospheric pressure changes from day to day enough to mean that in differentconditions the needle might read slightly under 100% vac and then even slightlyover.

Even if you use the glycerine filled gauges that Fred's talking about then thiswill still be the case; glycerine is in there to stop the needle bouncing insituations where the pressure oscillates (not the case when you have acatch-pot acting as an air receiver) which can make the needle difficult toread. Glycerine filled gauges are much less prone to damage though andso are certainly not without merit.

Sometimes, you'll also find that you get a tiny amount of 'stiction' on theneedle and a gentle tap on the gauge can re-correct the needle slightly.

Anyone, the bottom line is that if you're ready about 99% on a basic gauge andyour project is holding vacuum then you're good to go.

All the best, Matt



Matt Statham
Easy Composites / Carbon Mods - Technical Sales
fgayford
fgayford
Supreme Being (5.4K reputation)Supreme Being (5.4K reputation)Supreme Being (5.4K reputation)Supreme Being (5.4K reputation)Supreme Being (5.4K reputation)Supreme Being (5.4K reputation)Supreme Being (5.4K reputation)Supreme Being (5.4K reputation)Supreme Being (5.4K reputation)
Group: Forum Members
Posts: 433, Visits: 1.2K
111mattin111 (07/02/2016)
HI guys for some reason my pump doesn't seem to be pulling full vaccum, the flow indicator has stopped spinning but the gauge isn't quite at -30
Even with the part clamped off it still doesn't go down to -30 but it did used too what's causing this?  http://www.talkcomposites.com/Uploads/Images/cdb0d1a9-5c6b-429c-a415-f8ce.jpg


Hello
I used to use cheap gauges like this. I got rid of all of them and bought some really good liquid filled ones and the problem disappeared.
Fred
seense
seense
Supreme Being (139 reputation)Supreme Being (139 reputation)Supreme Being (139 reputation)Supreme Being (139 reputation)Supreme Being (139 reputation)Supreme Being (139 reputation)Supreme Being (139 reputation)Supreme Being (139 reputation)Supreme Being (139 reputation)
Group: Forum Members
Posts: 10, Visits: 138
You also might want to check if your needle is still properly fixed to the pin. Mine came loose after multiple times degassing and swirling the pot around to pop the bubbles. Had the same issue and when I removed the plastic cover it appeared the needle slipped on the center pin. Fixed it with a tiny drop epoxy.
111mattin111
111mattin111
Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)Supreme Being (613 reputation)
Group: Forum Members
Posts: 67, Visits: 910
Thanks for the replies I thought the tone of the pump had changed but thought I'd ask to make sure 
MarkMK
MarkMK
Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)
Group: Forum Members
Posts: 338, Visits: 2K
As Hanaldo said, pretty soon you'll not need to rely on the spinning indicator, as the absence of any crackling from the pump should tell you when no more air is being drawn through it

You might also find slight differences in your gauge reading depending upon the atmospheric conditions
Edited 10 Years Ago by MarkMK
Hanaldo
Hanaldo
Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Analogue gauges are quite inaccurate. If you connected a digital vac gauge you would likely find you are at full vac. The easiest way to tell is the tone of your pump, it's very easy to hear when the pump isn't under load any more and you will quickly learn the sounds of your pump. 