As said a good rule of thumb is the resin will have a TG around the temperature you postcured it to, especially in the early stages since initial cure.

You will find with time, the TG will improve as some of the uncured resin naturally cures, however you are not going to achieve the full 180C Tg naturally no matter how long you leave it as there isn't enough energy at room temperature to achieve the full level of cure needed.

Hence we always recommend a full postcure to achieve the highest possible Tg and best mechanical properties.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
thanasiss3
thanasiss3
Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)
Group: Forum Members
Posts: 18, Visits: 348
With this epoxy i have the tds so i can follow this and not try and error like the other i used!
Dravis
Dravis
Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)
Group: Forum Members
Posts: 592, Visits: 1.9K
I have postcured the EC high Temp resin at 90 -100 deg on several occasions .. when left for some time (weeks) after the postcure, my samples were above 130 deg. Tg

To ENSURE any given Tg  you must ramp up to the Tg you want .... following the TDS sheet.

 

"Sapere Aude"... Dare to KNOW!

The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...

103% of all people do not understand statistics...

Do not adjust our mind, theres a fault in reality :-)
thanasiss3
thanasiss3
Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)
Group: Forum Members
Posts: 18, Visits: 348
I found the tds sheet,they say you can partial post cure the system but i ask if someone know or ever try the partial cure,i want this info cause i need the higher tg at this post cure,i cannot raise the temp because i have the pastic cores under the carbon lamination,so i m looking to find if this high temp system can achieve a better tg after post curing at 70,than other usual laminating systems
Matthieu Libeert
Matthieu Libeert
Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
you can find everything you need in the technical data sheet of every product on the product page Smile 
here's the link to help you out http://www.easycomposites.co.uk/downloads/TDS/EC-TDS-Very-High-Temperature-Laminating-Resin.pdf
So to answer your question as well the Tg will probably be close to the temperature you've postcured your part or just a little bit above.
Sure the all-knowing compositesmaster Warren will be able to give you a more precise answer Wink

Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




thanasiss3
thanasiss3
Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)Supreme Being (116 reputation)
Group: Forum Members
Posts: 18, Visits: 348
Hello everyone,anybody knows if the easycompoaites very high temp epoxy can partial post cured at 60-70c?what will be the Tg?
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search