> We were using fiberglast system 2000
I don't know this resin, but I assume it is a normal laminating resin. What is its viscosity, in numbers? Is it low enough for infusion? If it doesn't specifically say infusion resin it probably isn't thin enough, especially not for larger parts. This can work for some infusion projects when used with slower hardeners, but often it doesn't.
> with 20 min epoxy hardener.
There you have it. Infusing a 20 minute resin for 35 minutes... it probably started to increase its viscosity even more before it had a chance to infuse the whole part. 20 minutes is too fast for this, you probably used up half of its pot life by mixing and degassing it.
|