gelcoat wrinkled over plastic


Author
Message
mrmarshal666
mrmarshal666
Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)
Group: Forum Members
Posts: 7, Visits: 53
Hi all!

I am new in this forum and also in Fiberglass part making!
 Today I did apply first time gel coat on my project hood! and gel coat did wrinkle up in some areas!

Hood is clear coated, polished and waxed many times with easycomposites.co.uk mold release wax.

Gel coat is mixed with 2% of hardener!



Attachments
IMG_20140103_175158.jpg (319 views, 904.00 KB)
IMG_20140103_175144.jpg (333 views, 911.00 KB)
IMG_20131230_182658.jpg (317 views, 1.00 MB)
ajb100
ajb100
Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)
Group: Forum Members
Posts: 346, Visits: 4.4K
In the third pic, where it has wrinkled, was it the black stuff?
Shaneer22
Shaneer22
Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)
Group: Forum Members
Posts: 156, Visits: 14K
Was the clear coat two pack.
mrmarshal666
mrmarshal666
Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)
Group: Forum Members
Posts: 7, Visits: 53
yes it has wrinkled only over black part! weird, i have coated all hood with clear coat!
mrmarshal666
mrmarshal666
Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)
Group: Forum Members
Posts: 7, Visits: 53
2k clear coat
Shaneer22
Shaneer22
Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)Supreme Being (1.1K reputation)
Group: Forum Members
Posts: 156, Visits: 14K
The gel coat has attacked,reacted with the clear coat I've had it once I put it down to not leaving the clear coat long enough to cure before applying release agents.
mrmarshal666
mrmarshal666
Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)
Group: Forum Members
Posts: 7, Visits: 53
My clear coat is applied 7 days ago!

carbonfibreworks
carbonfibreworks
Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)
Group: Forum Members
Posts: 292, Visits: 4.5K
How did your cure the 2k?
Chris
www.carbonfibreworks.co.uk

http://www.talkcomposites.com/Uploads/Images/97e08777-693c-4af1-a27a-86cf.png
mrmarshal666
mrmarshal666
Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)
Group: Forum Members
Posts: 7, Visits: 53
Peoples, have you all looked on pictures, before write any comments????

How can it be coating problem if gelcoat has lifted up in specific places, in straight lines .!!!
carbonfibreworks
carbonfibreworks
Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)
Group: Forum Members
Posts: 292, Visits: 4.5K
mrmarshal666 (04/01/2014)
Peoples, have you all looked on pictures, before write any comments????

How can it be coating problem if gelcoat has lifted up in specific places, in straight lines .!!!



Yes i  have looked at the images thank you and had a similar issue and that's why i asked the question above.
Chris 
www.carbonfibreworks.co.uk

http://www.talkcomposites.com/Uploads/Images/97e08777-693c-4af1-a27a-86cf.png
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search