Hi all!

I am new in this forum and also in Fiberglass part making!
 Today I did apply first time gel coat on my project hood! and gel coat did wrinkle up in some areas!

Hood is clear coated, polished and waxed many times with easycomposites.co.uk mold release wax.

Gel coat is mixed with 2% of hardener!



Attachments
IMG_20140103_175158.jpg (320 views, 904.00 KB)
IMG_20140103_175144.jpg (334 views, 911.00 KB)
IMG_20131230_182658.jpg (318 views, 1.00 MB)
Replies
carbonfibreworks
carbonfibreworks
Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)
Group: Forum Members
Posts: 292, Visits: 4.5K
How did your cure the 2k?
Chris
www.carbonfibreworks.co.uk

http://www.talkcomposites.com/Uploads/Images/97e08777-693c-4af1-a27a-86cf.png
mrmarshal666
mrmarshal666
Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)Forum Member (35 reputation)
Group: Forum Members
Posts: 7, Visits: 53
Peoples, have you all looked on pictures, before write any comments????

How can it be coating problem if gelcoat has lifted up in specific places, in straight lines .!!!
carbonfibreworks
carbonfibreworks
Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)
Group: Forum Members
Posts: 292, Visits: 4.5K
mrmarshal666 (04/01/2014)
Peoples, have you all looked on pictures, before write any comments????

How can it be coating problem if gelcoat has lifted up in specific places, in straight lines .!!!



Yes i  have looked at the images thank you and had a similar issue and that's why i asked the question above.
Chris 
www.carbonfibreworks.co.uk

http://www.talkcomposites.com/Uploads/Images/97e08777-693c-4af1-a27a-86cf.png
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
mrmarshal666 - 11 Years Ago
ajb100 - 11 Years Ago
mrmarshal666 - 11 Years Ago
Shaneer22 - 11 Years Ago
             2k clear coat
mrmarshal666 - 11 Years Ago
Shaneer22 - 11 Years Ago
             My clear coat is applied 7 days ago!
mrmarshal666 - 11 Years Ago
carbonfibreworks - 11 Years Ago
mrmarshal666 - 11 Years Ago
carbonfibreworks - 11 Years Ago
FLD - 11 Years Ago
carbonfibreworks - 11 Years Ago
mrmarshal666 - 11 Years Ago
Redline Fibreglass - 11 Years Ago
Redline Fibreglass - 11 Years Ago
andygtt - 11 Years Ago
mrmarshal666 - 11 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search