Hi,
I have just infused some carbon with IN2 resin but I poured 350g of resin and then added slow hardener for 250g. (75g instead of 105g) Will it ever set?

Brian.

I have just found that what was left in the mixing cup has set so I am feeling hopeful.
Edited 12 Years Ago by Brian_s
Reply
Warren (Staff)
Warren (Staff)
Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
You might be lucky as its not too massively out.  The more heat you can get into the part the better.

You may find a bit of a greasy surface once demoulded which will be some of the amines in the unused hardener coming to the surface.  you should be able to sand that out and polish it up.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...





Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search