By Brian_s - 10/18/2013 8:56:33 AM

Hi,
I have just infused some carbon with IN2 resin but I poured 350g of resin and then added slow hardener for 250g. (75g instead of 105g) Will it ever set?

Brian.

I have just found that what was left in the mixing cup has set so I am feeling hopeful.
By Warren (Staff) - 10/18/2013 12:32:13 PM

You might be lucky as its not too massively out.  The more heat you can get into the part the better.

You may find a bit of a greasy surface once demoulded which will be some of the amines in the unused hardener coming to the surface.  you should be able to sand that out and polish it up.