Leew
posted 12 Years Ago
ANSWER
HOT
Topic Details
Group: Forum Members
Posts: 33,
Visits: 187
I applied some coating resin to a part about 2 weeks ago. and even now it is still slighlty tacky to the touch. Weirdly the excess resin in the mixing pot seems to have cured fully and is not tacky. I used a digital scale and am pritty sure I mixed it 2:1. The part is made from glass cloth and EL1 laminating resin.
Any idea what could be the cause of the tackyness, and any way I could salvage the part? It took me quite some time to make the part so I'd really hate to have to toss it.
Edited
12 Years Ago by
Leew
Reply
Like
3
Replies
Leew
Leew
posted 12 Years Ago
ANSWER
HOT
Post Details
Group: Forum Members
Posts: 33,
Visits: 187
Anyone have any clue why my resin on the part has not cured properly. I think I'm going to have to toss the part and start again which is a bummer but I don't want to have the same problem again.
Reply
Like
3
fgayford
fgayford
posted 12 Years Ago
ANSWER
HOT
Post Details
Group: Forum Members
Posts: 433,
Visits: 1.2K
Leew (02/06/2013)
Anyone have any clue why my resin on the part has not cured properly. I think I'm going to have to toss the part and start again which is a bummer but I don't want to have the same problem again.
You have eliminated the temperature suspect so the only thing that remains is that you didn't get the mixture ratios correct.
Epoxy shows no mercy when mixing is not right on. Its even harder to get it right in small mixes. I know I have done it my self. I am now mixing to the 1/10 of a gram religiously and have not had a repeat of this problem.
Hope this helps.
Fred
Reply
Like
3
GO
Merge Selected
Merge into selected topic...
Merge into merge target...
Merge into a specific topic ID...
Open Merge
Threaded View
Threaded View
Coating resin still tacky after 2 weeks?
Leew
-
12 Years Ago
what temperature are you curing that part? must be over 15C° at least!
matthieutje65
-
12 Years Ago
I left it in the workshop which was about 10-15 degrees and then after a few days I left it on a rad...
Leew
-
12 Years Ago
Anyone have any clue why my resin on the part has not cured properly. I think I'm going to have to...
Leew
-
12 Years Ago
[quote][b]Leew (02/06/2013)[/b][hr]Anyone have any clue why my resin on the part has not cured...
fgayford
-
12 Years Ago
Even though I was pritty sure I mixed it right, perhaps I accidentally mixed it 5:1 which is the...
Leew
-
12 Years Ago
Dear Leew, when you apply a surface coat like this,the resin does not have enough volume in order to...
Nimateck
-
12 Years Ago
Post Reply
Like
3
Similar Topics
Post Quoted Reply
Reading This Topic
Login
Login
Remember Me
Reset Password
Resend Validation Email
Login
Facebook
Google
Explore
Messages
Mentions
Search