Hmmmm

So tried this, didn't quite go as per theory. I think it was because of not putting up proper barriers around the edges etc and I couldn't get the new part to fit, so just built it all up in filler.

Still a work in progress, need to do all the bodywork then start taking moulds... That'll be fun!

Cheers

Steven
tauruck
tauruck
Forum Guru (61 reputation)Forum Guru (61 reputation)Forum Guru (61 reputation)Forum Guru (61 reputation)Forum Guru (61 reputation)Forum Guru (61 reputation)Forum Guru (61 reputation)Forum Guru (61 reputation)Forum Guru (61 reputation)
Group: Forum Members
Posts: 7, Visits: 5
Good advice Fred, You saved him a mountain of work. Mike.
Steven
Steven
Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)
Group: Forum Members
Posts: 3, Visits: 127
Fred

That sounds like a much better plan! Thanks so much for sharing, I'll try this as per your advice.

I'll post the results up here 

Cheers

Steven
fgayford
fgayford
Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)
Group: Forum Members
Posts: 433, Visits: 1.2K
Hi Steven
I have done this many times. The answer is bondo. (that's what we call it here in Canada, its polyester based automotive body filler.)
Carefully in tomb the plasticine with bondo. Better tape off surrounding areas and wax over the tape. When you apply the bondo do it in layers, the first coat should be applied so as to capture the shape. Go past the shape to allow a flange around your piece about 2 inches. Once you have it about a inch thick you should have no trouble pulling it off.
Now dig out the plasticine and clean up any ragged edges.
So what you have is a rough mold. Wax many times and apply a number of coats of PVA. Apply a number of layers of bondo into your mold. I keep applying bondo in layers while there is still exotherm heat being given off. (just warm to the touch) Once filled to the desired thickness I pry the piece out of the mold while still warm. The reason I do this is that the bondo has not cured so hard that it will not break free from any little under cut craters, because this is a rough casting. The bondo is in a firm cheese state and will pop out easily.
Now you have a hard part that replaced the plasticene. Fit it to your part and you now you have a hard part that can be shaped into your mockup.
Hope this helps.
Fred     
Steven
Steven
Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)
Group: Forum Members
Posts: 3, Visits: 127
Hi Guys

So I mocked up a section that I want to fill in where the wheelarch meets the sill. The whole side will then be used as a plug to make a mould.

The problem I now have is that whilst I've a rough shape now of the section in plasticine I really need to sand and fine shape it but can't given it's plasticine. Was thinking of taking a mould of this small section, then making in FG, attaching then sanding and filling the FG piece - but this seems like a lot of hassle.

Are there any tricks I'm missing?

http://www.talkcomposites.com/Uploads/Images/3cb302d2-e670-4613-965e-943d.jpg




Thanks

Steven
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search