How to Make a Carbon Fiber Car Bonnet/Hood - Complete Guide


Author
Message
Matt (Staff)
Matt (Staff)
Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)Composites Expert (Staff) (11K reputation)
Group: Forum Members
Posts: 680, Visits: 1.9K
Hi Andy,

A post-cure in the mould would be a very good thing to do to ensure that there is no danger of the part distorting. 60'C for 6hrs would be a good post cure, after that there should be no danger of the part distorting in the sun.

If you need to post cure out of the mould then the recommendation would be to increase the temperature very gradually over  along period of time. This will reduce the amount of out of mould distortion.

All the best, Matt

Matt Statham
Easy Composites / Carbon Mods - Technical Sales
Warren (Staff)
Warren (Staff)
Supreme Being (31K reputation)Supreme Being (31K reputation)Supreme Being (31K reputation)Supreme Being (31K reputation)Supreme Being (31K reputation)Supreme Being (31K reputation)Supreme Being (31K reputation)Supreme Being (31K reputation)Supreme Being (31K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Another idea if your parts are too big for an oven is a modern temperature regulated heat blanket. I used one when I first made a bonnet at home and it achieved a mould surface temperature of 40 Celcius when placed on the complete infused mould layup, then wrapped in a duvet to reduce heat loss.

Although modern electric blankets have a thermal cut out and are designed to be left unsupervised, I would always recommend keeping a close eye on it as it isnt being used as the manufacturer intended.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
Extreme
Extreme
Supreme Being (157 reputation)Supreme Being (157 reputation)Supreme Being (157 reputation)Supreme Being (157 reputation)Supreme Being (157 reputation)Supreme Being (157 reputation)Supreme Being (157 reputation)Supreme Being (157 reputation)Supreme Being (157 reputation)
Group: Forum Members
Posts: 17, Visits: 78
Matt,

Can you please tell me why in your video you use GC50 Epoxy Compatible Ployester Gelcoat and not just your regular Clear Epoxy Gelcoat ?

thank you,

Erick
beer401
beer401
Junior Member (13 reputation)Junior Member (13 reputation)Junior Member (13 reputation)Junior Member (13 reputation)Junior Member (13 reputation)Junior Member (13 reputation)Junior Member (13 reputation)Junior Member (13 reputation)Junior Member (13 reputation)
Group: Forum Members
Posts: 1, Visits: 7
Dear Matt
My name is Weera .I am in Thailand.
Your video inspired me work the carbon hood.
I want to make he mold for resin infusion technique.
I can not find the good source compare to to yours.
Question
1.If I brush gelcoat , the infused resin to make the mold?
Bcoz sale person recommend me to spay gelcoat to avoid the league.

2.If I brush the gelcoat , then hand lay=up as you do.
How many hood that I can make from the mold?
What is your advised Matt...
Thank you for Matt and anyone who advised me.