Diolen epoxy lamination is first to fail in peel test


Author
Message
Lester Populaire
L
Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)Supreme Being (4.5K reputation)
Group: Forum Members
Posts: 311, Visits: 13K
The Mould Destroyer - 5/18/2021 4:33:12 PM
A quick update:



I did another test:
Changed Epoxy ratio from 100/60 to 100/50
4 variations:
2 400gm
2 200gm
one set in room temp (25)
one set on the 3d printer heated bad (55)

on the left is the heated one, on the right is the room temp

Heated one had a wood failor which is the optimal result, but there is a spot on the corner where the lamination failed, how weird is that

Anyway, The Epoxy is probably the problem doesn't cure well enough in room temp or something

Careful with your mixing ratio there. Epoxies require quite precisely measured ratios to fully polymerize. Unlike some other resins where the hardener is a catalyst that just starts a chain reaction within the monomer, in an epoxy you need both components to crosslink.
So stick as precisely as you can to the manufacturers instructions!

The Mould Destroyer
The Mould Destroyer
Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)
Group: Forum Members
Posts: 21, Visits: 332
Lester Populaire - 5/18/2021 7:51:55 PM
The Mould Destroyer - 5/18/2021 4:33:12 PM
A quick update:



I did another test:
Changed Epoxy ratio from 100/60 to 100/50
4 variations:
2 400gm
2 200gm
one set in room temp (25)
one set on the 3d printer heated bad (55)

on the left is the heated one, on the right is the room temp

Heated one had a wood failor which is the optimal result, but there is a spot on the corner where the lamination failed, how weird is that

Anyway, The Epoxy is probably the problem doesn't cure well enough in room temp or something

Careful with your mixing ratio there. Epoxies require quite precisely measured ratios to fully polymerize. Unlike some other resins where the hardener is a catalyst that just starts a chain reaction within the monomer, in an epoxy you need both components to crosslink.
So stick as precisely as you can to the manufacturers instructions!

Yes of course, the 100/50 was recommended by the seller 

Rosta Spicl
Rosta Spicl
Supreme Being (832 reputation)Supreme Being (832 reputation)Supreme Being (832 reputation)Supreme Being (832 reputation)Supreme Being (832 reputation)Supreme Being (832 reputation)Supreme Being (832 reputation)Supreme Being (832 reputation)Supreme Being (832 reputation)
Group: Forum Members
Posts: 54, Visits: 250
I recommend don't use lamination epoxy for bonding aplications. Use Epoxy based, 2K-PUR, MMA or MMA hybrid glues...the best for all the laminates bonding. I use these for high load constructions and it works great...

Warren (Staff)
Warren (Staff)
Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Certainly I would Agree, go for a proper structural adhesive every time for bonding applications like this as the bond strength, especially for relatively small bonding surface areas, is much stronger.

If you were just bonding two large sheets together with only light structural expectations, then yes a resin over such a large surface area is probably strong enough.  But for smaller areas, a dedicated structural adhesive will out perform a laminating resin.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
The Mould Destroyer
The Mould Destroyer
Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)
Group: Forum Members
Posts: 21, Visits: 332
Warren (Staff) - 5/20/2021 8:28:36 AM
Certainly I would Agree, go for a proper structural adhesive every time for bonding applications like this as the bond strength, especially for relatively small bonding surface areas, is much stronger.

If you were just bonding two large sheets together with only light structural expectations, then yes a resin over such a large surface area is probably strong enough.  But for smaller areas, a dedicated structural adhesive will out perform a laminating resin.

Thank you!
Just to clarify - the bonding is not the issue as is the laminated epoxy separating from the fabric
For bonding - I will preform a peel test on a lot of different glues to see which one will be the best

Warren (Staff)
Warren (Staff)
Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
I do wonder if there is any legs in testing abrading a bit deeper in your case?  almost down to the fabric.  

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
The Mould Destroyer
The Mould Destroyer
Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)
Group: Forum Members
Posts: 21, Visits: 332
Warren (Staff) - 5/24/2021 12:03:50 PM
I do wonder if there is any legs in testing abrading a bit deeper in your case?  almost down to the fabric.  

Sorry,
Can you elaborate a bit more?
Didn't understand the sentence

Hanaldo
Hanaldo
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
He means rather than bonding to the peel ply surface on the laminate, sand the laminate with 80 or 120 grit paper quite harshly until just before you hit the Diolen. 
Warren (Staff)
Warren (Staff)
Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Exactly Hanaldo,  It might make a bit of a difference.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
The Mould Destroyer
The Mould Destroyer
Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)Supreme Being (319 reputation)
Group: Forum Members
Posts: 21, Visits: 332
Hanaldo - 5/25/2021 11:28:29 PM
He means rather than bonding to the peel ply surface on the laminate, sand the laminate with 80 or 120 grit paper quite harshly until just before you hit the Diolen. 

Thanks!
I'ts a 2x 4 meters strip so its not practical for the current parts im building 

I switched to Kwik Kick and peel test came out great with the wood failing at a much higher peel force, with no heat, and a few hours set time to flip projects faster!


Now I have to figure out the best glue / adhesive / secondary bonding agent
There are so many options that I am so lost, and someone here mantined MMA and other stuff which threw me off even further

Edited 5 Years Ago by The Mould Destroyer