Structural analysis ,material properties


Author
Message
Gaurav Kumar Thakur
G
Supreme Being (164 reputation)Supreme Being (164 reputation)Supreme Being (164 reputation)Supreme Being (164 reputation)Supreme Being (164 reputation)Supreme Being (164 reputation)Supreme Being (164 reputation)Supreme Being (164 reputation)Supreme Being (164 reputation)
Group: Forum Members
Posts: 9, Visits: 273
Hi
I have done component using CFRP prepreg now i wanted to FEA analysis for the same ,Vendor has provided the technical data sheet for the same but in that only three properties are given ,tensile modulus,Tensile strength ,and %elongation, can any body give suggestion what should be done??? 
Reply
Rosta Spicl
Rosta Spicl
Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)
Group: Forum Members
Posts: 54, Visits: 250
Not easy...
Fibre based composites are strictly transversely isothropic. For structural static analysis the must have parameter is Young modulus for 0° (E1) and 90° (E2). For wooven fabrics boths are the same, not for UDs...there is the E2 cca 10-15x lower than E1. Remember, the E is largely different for dry fibres and cured laminate.
The FEM model has to be strictly the same like a real sample, the plies schedule, fibers direction, thickness etc. I´d recommend the fem model build like a shell.
The best is validate the FEM model with reality, measure the displacement and stresses on real condicions and fit it on FEM model.
Good luck, FEM on complex composites structures is the big chalange...

GO