Hello to all!

I'm new to composites and diving in!

I would like your suggestion on making 2 sided glossy GF plates. 1mm to 6 mm

I did start a test of infusion in between 2 glass panels that are waxed. Am I off track oy not?

What do production shops do?

Thanks
Reply
Rosta Spicl
Rosta Spicl
Supreme Being (574 reputation)Supreme Being (574 reputation)Supreme Being (574 reputation)Supreme Being (574 reputation)Supreme Being (574 reputation)Supreme Being (574 reputation)Supreme Being (574 reputation)Supreme Being (574 reputation)Supreme Being (574 reputation)
Group: Forum Members
Posts: 54, Visits: 250
Prepregs, no other way. I have tried a plates made of polished aluminium sheets thk of 12mm instead glass, vacuumed, pressed in autoclave +8bar, baked. The result was great, but needs a lot of experience and technology.
The 2-shot process like Hanaldo talking about is quite OK, but you have to bond it together in jig plates as well to keep constant thickness.