Second mold, new issues :-)


Author
Message
Massimiliano
M
Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)
Group: Forum Members
Posts: 167, Visits: 1.1K
Hi, after the first not successful mold and part (http://www.talkcomposites.com/Topic36543.aspx) I worked on the part to fix the issues in order to build a new mold.
This time the part popped from the mold almost by itself but... something has happened to the tooling gelcoat!
Please se pics. Last pic is the tooling gelcoat on the base glass, so I tend to exclude some interaction with the plug.
Any ideas?


Attachments
20200814_151808.jpg (365 views, 1.00 MB)
20200814_152504.jpg (340 views, 2.00 MB)
Replies
Massimiliano
M
Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)
Group: Forum Members
Posts: 167, Visits: 1.1K
beliblisk - 8/16/2020 6:59:44 PM
Massimiliano - 8/16/2020 6:54:06 PM
Massimiliano - 8/14/2020 4:31:52 PM
Warren (Staff) - 8/14/2020 4:28:41 PM
If you look at your second attached image, you can see the strands of fibreglass heavily printing through the flat gelcoat to the right.  That might be a side effect of the reaction you have had but looking to the left and edge of the mould it doesn't look much better.

It might be pre-release from the surface in some way as the edge looks a bit like the gel has distorted a bit but that doesn't account for all of it.

Thanks... hope my third mold would be better :-)

Do you have any suggestions on how to fix this mold?

Anyone has suggestion on how to fix this problem?
Just apply new gelcoat?
Is there any way to apply it the "flattest" possible?

I think the fastes way would be to redo whole mould from scratch. 1% catalysts seems way to low for gelcoat (i always go with 2%). Peehaps first layer didnt cure and then second layer pulled it a bit.

If you were to try and fix it there will be a lot of sanding:/
Apply gelocat with spatula and cover it with flash tape so you will get relatively flat surface..... sand and do one more step if any low spots remain.

Thank you... I will try on one damaged area and see how it will go... then decide to redo it for the third time..๐Ÿ˜’

beliblisk
b
Supreme Being (813 reputation)Supreme Being (813 reputation)Supreme Being (813 reputation)Supreme Being (813 reputation)Supreme Being (813 reputation)Supreme Being (813 reputation)Supreme Being (813 reputation)Supreme Being (813 reputation)Supreme Being (813 reputation)
Group: Forum Members
Posts: 53, Visits: 2.8K
Massimiliano - 8/16/2020 7:05:56 PM
beliblisk - 8/16/2020 6:59:44 PM
Massimiliano - 8/16/2020 6:54:06 PM
Massimiliano - 8/14/2020 4:31:52 PM
Warren (Staff) - 8/14/2020 4:28:41 PM
If you look at your second attached image, you can see the strands of fibreglass heavily printing through the flat gelcoat to the right.  That might be a side effect of the reaction you have had but looking to the left and edge of the mould it doesn't look much better.

It might be pre-release from the surface in some way as the edge looks a bit like the gel has distorted a bit but that doesn't account for all of it.

Thanks... hope my third mold would be better :-)

Do you have any suggestions on how to fix this mold?

Anyone has suggestion on how to fix this problem?
Just apply new gelcoat?
Is there any way to apply it the "flattest" possible?

I think the fastes way would be to redo whole mould from scratch. 1% catalysts seems way to low for gelcoat (i always go with 2%). Peehaps first layer didnt cure and then second layer pulled it a bit.

If you were to try and fix it there will be a lot of sanding:/
Apply gelocat with spatula and cover it with flash tape so you will get relatively flat surface..... sand and do one more step if any low spots remain.

Thank you... I will try on one damaged area and see how it will go... then decide to redo it for the third time..๐Ÿ˜’

You are welcome. I tend to take every failure as a learning process...... just keep it up and you will get there eventuallySmile 

Massimiliano
M
Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)
Group: Forum Members
Posts: 167, Visits: 1.1K
beliblisk - 8/16/2020 7:11:15 PM
Massimiliano - 8/16/2020 7:05:56 PM
beliblisk - 8/16/2020 6:59:44 PM
Massimiliano - 8/16/2020 6:54:06 PM
Massimiliano - 8/14/2020 4:31:52 PM
Warren (Staff) - 8/14/2020 4:28:41 PM
If you look at your second attached image, you can see the strands of fibreglass heavily printing through the flat gelcoat to the right.  That might be a side effect of the reaction you have had but looking to the left and edge of the mould it doesn't look much better.

It might be pre-release from the surface in some way as the edge looks a bit like the gel has distorted a bit but that doesn't account for all of it.

Thanks... hope my third mold would be better :-)

Do you have any suggestions on how to fix this mold?

Anyone has suggestion on how to fix this problem?
Just apply new gelcoat?
Is there any way to apply it the "flattest" possible?

I think the fastes way would be to redo whole mould from scratch. 1% catalysts seems way to low for gelcoat (i always go with 2%). Peehaps first layer didnt cure and then second layer pulled it a bit.

If you were to try and fix it there will be a lot of sanding:/
Apply gelocat with spatula and cover it with flash tape so you will get relatively flat surface..... sand and do one more step if any low spots remain.

Thank you... I will try on one damaged area and see how it will go... then decide to redo it for the third time..๐Ÿ˜’

You are welcome. I tend to take every failure as a learning process...... just keep it up and you will get there eventuallySmile 

Yes you are right, first mold plug did not release properly as there were some slight undercuts. Also while applying the tooling resin I mixed too much in one pot so it started to gel before finishing to apply the various layer of mat ๐Ÿคฆโ€โ™‚๏ธ

beliblisk
b
Supreme Being (813 reputation)Supreme Being (813 reputation)Supreme Being (813 reputation)Supreme Being (813 reputation)Supreme Being (813 reputation)Supreme Being (813 reputation)Supreme Being (813 reputation)Supreme Being (813 reputation)Supreme Being (813 reputation)
Group: Forum Members
Posts: 53, Visits: 2.8K
Massimiliano - 8/16/2020 7:19:15 PM
beliblisk - 8/16/2020 7:11:15 PM
Massimiliano - 8/16/2020 7:05:56 PM
beliblisk - 8/16/2020 6:59:44 PM
Massimiliano - 8/16/2020 6:54:06 PM
Massimiliano - 8/14/2020 4:31:52 PM
Warren (Staff) - 8/14/2020 4:28:41 PM
If you look at your second attached image, you can see the strands of fibreglass heavily printing through the flat gelcoat to the right.  That might be a side effect of the reaction you have had but looking to the left and edge of the mould it doesn't look much better.

It might be pre-release from the surface in some way as the edge looks a bit like the gel has distorted a bit but that doesn't account for all of it.

Thanks... hope my third mold would be better :-)

Do you have any suggestions on how to fix this mold?

Anyone has suggestion on how to fix this problem?
Just apply new gelcoat?
Is there any way to apply it the "flattest" possible?

I think the fastes way would be to redo whole mould from scratch. 1% catalysts seems way to low for gelcoat (i always go with 2%). Peehaps first layer didnt cure and then second layer pulled it a bit.

If you were to try and fix it there will be a lot of sanding:/
Apply gelocat with spatula and cover it with flash tape so you will get relatively flat surface..... sand and do one more step if any low spots remain.

Thank you... I will try on one damaged area and see how it will go... then decide to redo it for the third time..๐Ÿ˜’

You are welcome. I tend to take every failure as a learning process...... just keep it up and you will get there eventuallySmile 

Yes you are right, first mold plug did not release properly as there were some slight undercuts. Also while applying the tooling resin I mixed too much in one pot so it started to gel before finishing to apply the various layer of mat ๐Ÿคฆโ€โ™‚๏ธ

Gealcoat wont gel on you to fast opposed to coupling coat and tooling resin (with both of these i go just above lower limit for catalyst and mix amounts i can use in the next few minutes).

When making the plug and filling stuff with fileting wax always think how you will make cf part (either to help easy release of making your life easier laying carbon cloth). It may look straight forward but it actually sometimes takes a lot of forward thinkingSmile

Massimiliano
M
Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)
Group: Forum Members
Posts: 167, Visits: 1.1K
beliblisk - 8/16/2020 7:25:39 PM
Massimiliano - 8/16/2020 7:19:15 PM
beliblisk - 8/16/2020 7:11:15 PM
Massimiliano - 8/16/2020 7:05:56 PM
beliblisk - 8/16/2020 6:59:44 PM
Massimiliano - 8/16/2020 6:54:06 PM
Massimiliano - 8/14/2020 4:31:52 PM
Warren (Staff) - 8/14/2020 4:28:41 PM
If you look at your second attached image, you can see the strands of fibreglass heavily printing through the flat gelcoat to the right.  That might be a side effect of the reaction you have had but looking to the left and edge of the mould it doesn't look much better.

It might be pre-release from the surface in some way as the edge looks a bit like the gel has distorted a bit but that doesn't account for all of it.

Thanks... hope my third mold would be better :-)

Do you have any suggestions on how to fix this mold?

Anyone has suggestion on how to fix this problem?
Just apply new gelcoat?
Is there any way to apply it the "flattest" possible?

I think the fastes way would be to redo whole mould from scratch. 1% catalysts seems way to low for gelcoat (i always go with 2%). Peehaps first layer didnt cure and then second layer pulled it a bit.

If you were to try and fix it there will be a lot of sanding:/
Apply gelocat with spatula and cover it with flash tape so you will get relatively flat surface..... sand and do one more step if any low spots remain.

Thank you... I will try on one damaged area and see how it will go... then decide to redo it for the third time..๐Ÿ˜’

You are welcome. I tend to take every failure as a learning process...... just keep it up and you will get there eventuallySmile 

Yes you are right, first mold plug did not release properly as there were some slight undercuts. Also while applying the tooling resin I mixed too much in one pot so it started to gel before finishing to apply the various layer of mat ๐Ÿคฆโ€โ™‚๏ธ

Gealcoat wont gel on you to fast opposed to coupling coat and tooling resin (with both of these i go just above lower limit for catalyst and mix amounts i can use in the next few minutes).

When making the plug and filling stuff with fileting wax always think how you will make cf part (either to help easy release of making your life easier laying carbon cloth). It may look straight forward but it actually sometimes takes a lot of forward thinkingSmile

Definitely yes!
Thank you!

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
mporta71 - 6 Years Ago
Warren (Staff) - 6 Years Ago
mporta71 - 6 Years Ago
Warren (Staff) - 6 Years Ago
mporta71 - 6 Years Ago
mporta71 - 6 Years Ago
beliblisk - 6 Years Ago
mporta71 - 6 Years Ago
beliblisk - 6 Years Ago
mporta71 - 6 Years Ago
beliblisk - 6 Years Ago
                                         Definitely yes! Thank you!
mporta71 - 6 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search