Hey guys, novice here with some questions... I recently bought a front lip for my car which is made of unpainted polypropylene plastic.

Instead of making a fibreglass mould from it. Is it possible to laminate carbon fibre directly onto it after applying a release agent?

Would it damage the front lip if i remove the carbon fibre from it do you think?

Would these be the basics steps?:

- Release agent - single wax layer or single pva layer? or both? (wax layer and then pva layer) ? which is better
- epoxy resin layer
- wait til tacky
- carbon fibre cloth
- epoxy resin
- wait to fully cure
- sand low grit to high grit
- and then one last epoxy resin layer? wait to fully cure
- sand again low grit to high grit

how do i know when to stop applying layers of epoxy resin layers? until it’s completely smooth/flat?
and if another resin layer is added. does it end with sanding again or is the resin layer the last step?

does it then need a uv resistant clear coat because it’s exposed to the sun? or will the epoxy resin be enough?

do i then go ahead and use detailing compound/cut and polish/wax for the perfect glossy look?

thanks guys
Warren (Staff)
Warren (Staff)
Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
If it is smooth glossy polypropylene then epoxy resin will not stick to it, so demoulding should be quite easy. 

I suspect you would want more than 1 layer of cloth - a typical 210gsm cloth is around 4 layers per mm thickness.

If you follow our skinning video - in essence the resin build up process is the same, you would hit it with 3 coats then sand it flat.

Lacquer or polish is personal preference.  In very sunny or hot climates, a lacquer will offer more UV stability.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
kymearra
k
Junior Member (23 reputation)Junior Member (23 reputation)Junior Member (23 reputation)Junior Member (23 reputation)Junior Member (23 reputation)Junior Member (23 reputation)Junior Member (23 reputation)Junior Member (23 reputation)Junior Member (23 reputation)
Group: Forum Members
Posts: 2, Visits: 5
Warren (Staff) - 5/26/2020 3:37:10 PM
If it is smooth glossy polypropylene then epoxy resin will not stick to it, so demoulding should be quite easy. 

I suspect you would want more than 1 layer of cloth - a typical 210gsm cloth is around 4 layers per mm thickness.

If you follow our skinning video - in essence the resin build up process is the same, you would hit it with 3 coats then sand it flat.

Lacquer or polish is personal preference.  In very sunny or hot climates, a lacquer will offer more UV stability.

Hey Warren, thanks for the info. How many layers of CF would you recommend for a car front lip?

What would be the first thing you apply after applying the release mould?
Straight to the resin/hardener mix? and then lay your CF cloth?

Thanks
Warren (Staff)
Warren (Staff)
Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Depends on the shape and how big it is.  A shallow lip would only need around 4 layers.  A bigger lip with some curve to it or some angles/bends would be ok at that as the curves will add stiffness due to the shape.  If it is more splitter or sticks out far, then go for a foam core for weight reasons and added stiffness  -  we sell flat splitter panels ourselves but use a foam core with a couple of layers of fabric either side.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search