Making my own curved plywood/veneer with vacuum bagging


Author
Message
Antoine
Antoine
Junior Member (16 reputation)Junior Member (16 reputation)Junior Member (16 reputation)Junior Member (16 reputation)Junior Member (16 reputation)Junior Member (16 reputation)Junior Member (16 reputation)Junior Member (16 reputation)Junior Member (16 reputation)
Group: Forum Members
Posts: 2, Visits: 12
Hello guys,
I'm a wooden surfboard builder and I have the project to build some kitesurf boards like on the following pictures:



I'm not sure about which technique to use to glue those sheets of wood together with a curve and even some concaves (like a skateboard).
I have no experience at all in vacuum bagging but I thought of using a mold and vacuum bagging technique to glue them together. My questions are:
- Could you light me on the technique to use, or maybe send me a link to a tutorial for similar results.
- I'm thinking of buying the starters set with the vacuum pump? Would that be sufficient or do would I need extra material (I plan to glue either with PU glue or with epoxy)

Thank you so much for your help and greets from Portugal,
Antoine

Chris Rogers
C
Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)
Group: Forum Members
Posts: 120, Visits: 933
If you're not making a huge number, vacuum bagging would be easier than making a press.  Many ski and skateboard builders use shaped platens on large presses with either hydraulic or pneumatic (like inflated fire hose) clamps.  If you can make a simple curved form that holds vacuum then it will work fine.  You could make the shape from wood and glue a sheet of plastic or thin aluminum to make the air-tight surface.  

Here are two of my articles that might help:
(...could copy and paste but that would be a long post!)

Vacuum Bagging:

https://explorecomposites.com/articles/lamination/basics-vacuum-bagging/

Buying a Vacuum Pump:

https://explorecomposites.com/articles/tools-and-equipment/buying-a-vacuum-pump/

You probably don't need a high vacuum for this so a dry rotary vane, diaphragm or other cheap oil-free pump would be fine.  You won't regret having a nice one though if you plan to get into more composite work - just make sure you get a catch-pot too to protect it.  