I’m not sure what youre using the steel for. Is it to add rigidity to a mould or a finished part?
If for a mould, youll need to insulate the steel with E glass to protect it from the Carbon, OR, completely seal the steel off from any oxygen exposure to prevent galvanic corrosion.
Also, sand the steel with 40 or 50 grit paper thoroughly. Clean it in uni directional wipes with acetone multiple times. Using a swirling motion just spreads residual dirt and grease around the metal. Add the metal to the layup shortly after the acetone evaporates.
The foam idea sounds good. Is it needed though? Also are you using it to add structure or floatation? Use 2 pound foam for floatation, and 4 pound or higher if youre looking to add some rigidity.
Jason
|