Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)
Group: Forum Members
Posts: 680, Visits: 1.9K
Hi Javier,

There's only 3 things that could cause the epoxy to not cure properly:-

1) The mix ratio - you need to be really accurate with your measurements. Measure by weight, not volume. Aim to be acurate to 1g.
2) The thoroughness of the mixing - always ensure you spend lots of time to carefuly mix the epoxy and hardener together
3) The temperature where you're working - It is essential to maintain an ambient (workshop) temperature of 20'C or very close to 20'C. If the temperature becomes too low then the epoxy can slow down or stop curing altogether. I would suggest putting your part somewhere very warm to see if you can 'kick-start' the cure again.

Try heating the part up before you resort to stripping the uncured resin off.

--Matt

Matt Statham
Easy Composites / Carbon Mods - Technical Sales
javier
javier
Forum Guru (71 reputation)Forum Guru (71 reputation)Forum Guru (71 reputation)Forum Guru (71 reputation)Forum Guru (71 reputation)Forum Guru (71 reputation)Forum Guru (71 reputation)Forum Guru (71 reputation)Forum Guru (71 reputation)
Group: Forum Members
Posts: 7, Visits: 36
Hi,

Definitely the workshop temperature was the problem. I placed the paddle in a smaller room with a little electric heater and it worked perfectly.

Thank you again for your help.

Javier.
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search