Hello, I am casting my projects upside down on a smooth plastic, almost glass surface. I cast this way as I place my furniture pieces in the resin on my second or third pour ( curved wood). I notice a soon as I pour my first coat, a haze like film appears on the surface, almost seems to thicken instantly. It is only obvious at an angle initially. As the project cures, over a period of a few days this haze goes scally/off white and noticeable looking through the resin once removed from the mold and flipped over. As I have curved wood in the resin protruding out is is impossible to sand out/remove. How do I avoid this initial haze? I have attached two images. the close up is the image looking through the top, where you can see the white scales.


Edited 6 Years Ago by Randy Mugford
Replies
Rich (Staff)
Rich (Staff)
Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)
Group: Administrators
Posts: 167, Visits: 4.6K
Hi Randy, the concept of the table looks great and you should be able to get a perfect/flawless finish so we'd like you to get to the bottom of the cause of this problem. In the first instance, what type of plastic/material are you using as the mould surface? Does it self-release (like Polypropylene) or do you use a release agent; if you use a release agent, what type are you using?
Randy Mugford
R
Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)
Group: Forum Members
Posts: 7, Visits: 23
Rich (Staff) - 2/4/2019 5:35:01 PM
Hi Randy, the concept of the table looks great and you should be able to get a perfect/flawless finish so we'd like you to get to the bottom of the cause of this problem. In the first instance, what type of plastic/material are you using as the mould surface? Does it self-release (like Polypropylene) or do you use a release agent; if you use a release agent, what type are you using?

Thanks for the reply. No release agent is being used. I cast it on a very dense Polypropylene, almost glass finish. Releases easy. I apply on coat 1/4 inch thick, then after 12 hours place the wood structure in it, and pour 3 more coats each at about 1/2 inch. I never noticed it originally while pouring it, but after the job was complete the white scales started to show up and got more noticeable over time. Initially I thought it could be too much moisture, but the temp is at 22 and the moisture is very low. I noticed today after an initial pour of i/4 inch i had a film develop on about 20% of the surface ( only detectable at a certain angle) that was almost at a tacky stage after 10 minutes. I used a flat blade and removed the film, which them turned milky, and disposed of it. Problem is I cannot do this after I place the wood in. The eventual top side of the furniture piece has been and likely again will be flawless, it is the back side where the issue is, which is the side i am pour each layer on, as a result of doing the piece upside down.


Edited 6 Years Ago by Randy Mugford
Lester Populaire
L
Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)
Group: Forum Members
Posts: 311, Visits: 13K
Randy Mugford - 2/4/2019 6:42:41 PM
Rich (Staff) - 2/4/2019 5:35:01 PM
Hi Randy, the concept of the table looks great and you should be able to get a perfect/flawless finish so we'd like you to get to the bottom of the cause of this problem. In the first instance, what type of plastic/material are you using as the mould surface? Does it self-release (like Polypropylene) or do you use a release agent; if you use a release agent, what type are you using?

Thanks for the reply. No release agent is being used. I cast it on a very dense Polypropylene, almost glass finish. Releases easy. I apply on coat 1/4 inch thick, then after 12 hours place the wood structure in it, and pour 3 more coats each at about 1/2 inch. I never noticed it originally while pouring it, but after the job was complete the white scales started to show up and got more noticeable over time. Initially I thought it could be too much moisture, but the temp is at 22 and the moisture is very low. I noticed today after an initial pour of i/4 inch i had a film develop on about 20% of the surface ( only detectable at a certain angle) that was almost at a tacky stage after 10 minutes. I used a flat blade and removed the film, which them turned milky, and disposed of it. Problem is I cannot do this after I place the wood in. The eventual top side of the furniture piece has been and likely again will be flawless, it is the back side where the issue is, which is the side i am pour each layer on, as a result of doing the piece upside down.


That looks like amine blush type thing to me. I'd bet it is due to measuring inaccuracy or not well mixed resin. Big quantities can be hard to mix properly. 

Randy Mugford
R
Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)
Group: Forum Members
Posts: 7, Visits: 23
Lester Populaire - 2/4/2019 9:24:19 PM
Randy Mugford - 2/4/2019 6:42:41 PM
Rich (Staff) - 2/4/2019 5:35:01 PM
Hi Randy, the concept of the table looks great and you should be able to get a perfect/flawless finish so we'd like you to get to the bottom of the cause of this problem. In the first instance, what type of plastic/material are you using as the mould surface? Does it self-release (like Polypropylene) or do you use a release agent; if you use a release agent, what type are you using?

Thanks for the reply. No release agent is being used. I cast it on a very dense Polypropylene, almost glass finish. Releases easy. I apply on coat 1/4 inch thick, then after 12 hours place the wood structure in it, and pour 3 more coats each at about 1/2 inch. I never noticed it originally while pouring it, but after the job was complete the white scales started to show up and got more noticeable over time. Initially I thought it could be too much moisture, but the temp is at 22 and the moisture is very low. I noticed today after an initial pour of i/4 inch i had a film develop on about 20% of the surface ( only detectable at a certain angle) that was almost at a tacky stage after 10 minutes. I used a flat blade and removed the film, which them turned milky, and disposed of it. Problem is I cannot do this after I place the wood in. The eventual top side of the furniture piece has been and likely again will be flawless, it is the back side where the issue is, which is the side i am pour each layer on, as a result of doing the piece upside down.


That looks like amine blush type thing to me. I'd bet it is due to measuring inaccuracy or not well mixed resin. Big quantities can be hard to mix properly. 

Thank you. I will double my mix time and see what happens. I thought amine blush was a moisture reaction. I wondered if the heat gun caused the reaction. Once again thanks!

Matthieu Libeert
Matthieu Libeert
Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
Randy Mugford - 2/4/2019 9:32:30 PM
Lester Populaire - 2/4/2019 9:24:19 PM
Randy Mugford - 2/4/2019 6:42:41 PM
Rich (Staff) - 2/4/2019 5:35:01 PM
Hi Randy, the concept of the table looks great and you should be able to get a perfect/flawless finish so we'd like you to get to the bottom of the cause of this problem. In the first instance, what type of plastic/material are you using as the mould surface? Does it self-release (like Polypropylene) or do you use a release agent; if you use a release agent, what type are you using?

Thanks for the reply. No release agent is being used. I cast it on a very dense Polypropylene, almost glass finish. Releases easy. I apply on coat 1/4 inch thick, then after 12 hours place the wood structure in it, and pour 3 more coats each at about 1/2 inch. I never noticed it originally while pouring it, but after the job was complete the white scales started to show up and got more noticeable over time. Initially I thought it could be too much moisture, but the temp is at 22 and the moisture is very low. I noticed today after an initial pour of i/4 inch i had a film develop on about 20% of the surface ( only detectable at a certain angle) that was almost at a tacky stage after 10 minutes. I used a flat blade and removed the film, which them turned milky, and disposed of it. Problem is I cannot do this after I place the wood in. The eventual top side of the furniture piece has been and likely again will be flawless, it is the back side where the issue is, which is the side i am pour each layer on, as a result of doing the piece upside down.


That looks like amine blush type thing to me. I'd bet it is due to measuring inaccuracy or not well mixed resin. Big quantities can be hard to mix properly. 

Thank you. I will double my mix time and see what happens. I thought amine blush was a moisture reaction. I wondered if the heat gun caused the reaction. Once again thanks!

As above I would say moist related or temperature changes, unproper mixing, and now that you talk about heat gun, there is a big chance you "burned" your epoxy, if you leave your heatgun to long on a spot it will create a thin dull film. Could it also be that your wood is not completely dry? When I make my tables I leave the wood in an oven for over a week to remove any moist in the wood that might transfer into your resin when the resin goes exothermal and creates big temperatures causing the moist to "vape" into your resin causing bubbles and haze. 


Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




Randy Mugford
R
Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)
Group: Forum Members
Posts: 7, Visits: 23
Matthieu Libeert - 2/6/2019 7:05:35 PM
Randy Mugford - 2/4/2019 9:32:30 PM
Lester Populaire - 2/4/2019 9:24:19 PM
Randy Mugford - 2/4/2019 6:42:41 PM
Rich (Staff) - 2/4/2019 5:35:01 PM
Hi Randy, the concept of the table looks great and you should be able to get a perfect/flawless finish so we'd like you to get to the bottom of the cause of this problem. In the first instance, what type of plastic/material are you using as the mould surface? Does it self-release (like Polypropylene) or do you use a release agent; if you use a release agent, what type are you using?

Thanks for the reply. No release agent is being used. I cast it on a very dense Polypropylene, almost glass finish. Releases easy. I apply on coat 1/4 inch thick, then after 12 hours place the wood structure in it, and pour 3 more coats each at about 1/2 inch. I never noticed it originally while pouring it, but after the job was complete the white scales started to show up and got more noticeable over time. Initially I thought it could be too much moisture, but the temp is at 22 and the moisture is very low. I noticed today after an initial pour of i/4 inch i had a film develop on about 20% of the surface ( only detectable at a certain angle) that was almost at a tacky stage after 10 minutes. I used a flat blade and removed the film, which them turned milky, and disposed of it. Problem is I cannot do this after I place the wood in. The eventual top side of the furniture piece has been and likely again will be flawless, it is the back side where the issue is, which is the side i am pour each layer on, as a result of doing the piece upside down.


That looks like amine blush type thing to me. I'd bet it is due to measuring inaccuracy or not well mixed resin. Big quantities can be hard to mix properly. 

Thank you. I will double my mix time and see what happens. I thought amine blush was a moisture reaction. I wondered if the heat gun caused the reaction. Once again thanks!

As above I would say moist related or temperature changes, unproper mixing, and now that you talk about heat gun, there is a big chance you "burned" your epoxy, if you leave your heatgun to long on a spot it will create a thin dull film. Could it also be that your wood is not completely dry? When I make my tables I leave the wood in an oven for over a week to remove any moist in the wood that might transfer into your resin when the resin goes exothermal and creates big temperatures causing the moist to "vape" into your resin causing bubbles and haze. 

Thanks. I'll put this in point form to make it quicker ...
A.  The wood is kiln dried laminate, and has 4 coats water base finish (this haze is apparent without contacting the wood). B. With or without the heat gun, same effect. C. It is mixed for 10 plus minutes, in a clear container to insure proper mixing. About three cups mixed at a time, to lesson improper mixing. Room set at 22 degrees, humidity at 40%. The haze is immediately after pouring on about 25 % of the surface, and it is random. The surface area is 12 square feet, and the resin barely contacts the wood. The haze happens within the first minute. It is only noticeable a an angle with the the right light direction. I have learned after 15 pours now to lightly scrap it off after each pour . When you scrap it it immediately developed with strands, with micro bubbles in it. I basically scrap it to the edges now and remove it. Over 12 square feet it is a hassle. If I do not remove it, it becomes white -ish and scally looking after a few day, and is impossible to remove, or mask.Thanks for your help!! Much appreciated




Edited 6 Years Ago by Randy Mugford
Matthieu Libeert
Matthieu Libeert
Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
Randy Mugford - 2/6/2019 7:19:42 PM
Matthieu Libeert - 2/6/2019 7:05:35 PM
Randy Mugford - 2/4/2019 9:32:30 PM
Lester Populaire - 2/4/2019 9:24:19 PM
Randy Mugford - 2/4/2019 6:42:41 PM
Rich (Staff) - 2/4/2019 5:35:01 PM
Hi Randy, the concept of the table looks great and you should be able to get a perfect/flawless finish so we'd like you to get to the bottom of the cause of this problem. In the first instance, what type of plastic/material are you using as the mould surface? Does it self-release (like Polypropylene) or do you use a release agent; if you use a release agent, what type are you using?

Thanks for the reply. No release agent is being used. I cast it on a very dense Polypropylene, almost glass finish. Releases easy. I apply on coat 1/4 inch thick, then after 12 hours place the wood structure in it, and pour 3 more coats each at about 1/2 inch. I never noticed it originally while pouring it, but after the job was complete the white scales started to show up and got more noticeable over time. Initially I thought it could be too much moisture, but the temp is at 22 and the moisture is very low. I noticed today after an initial pour of i/4 inch i had a film develop on about 20% of the surface ( only detectable at a certain angle) that was almost at a tacky stage after 10 minutes. I used a flat blade and removed the film, which them turned milky, and disposed of it. Problem is I cannot do this after I place the wood in. The eventual top side of the furniture piece has been and likely again will be flawless, it is the back side where the issue is, which is the side i am pour each layer on, as a result of doing the piece upside down.


That looks like amine blush type thing to me. I'd bet it is due to measuring inaccuracy or not well mixed resin. Big quantities can be hard to mix properly. 

Thank you. I will double my mix time and see what happens. I thought amine blush was a moisture reaction. I wondered if the heat gun caused the reaction. Once again thanks!

As above I would say moist related or temperature changes, unproper mixing, and now that you talk about heat gun, there is a big chance you "burned" your epoxy, if you leave your heatgun to long on a spot it will create a thin dull film. Could it also be that your wood is not completely dry? When I make my tables I leave the wood in an oven for over a week to remove any moist in the wood that might transfer into your resin when the resin goes exothermal and creates big temperatures causing the moist to "vape" into your resin causing bubbles and haze. 

Thanks. I'll put this in point form to make it quicker ...
A.  The wood is kiln dried laminate, and has 4 coats water base finish (this haze is apparent without contacting the wood). B. With or without the heat gun, same effect. C. It is mixed for 10 plus minutes, in a clear container to insure proper mixing. About three cups mixed at a time, to lesson improper mixing. Room set at 22 degrees, humidity at 40%. The haze is immediately after pouring on about 25 % of the surface, and it is random. The surface area is 12 square feet, and the resin barely contacts the wood. The haze happens within the first minute. It is only noticeable a an angle with the the right light direction. I have learned after 15 pours now to lightly scrap it off after each pour . When you scrap it it immediately developed with strands, with micro bubbles in it. I basically scrap it to the edges now and remove it. Over 12 square feet it is a hassle. If I do not remove it, it becomes white -ish and scally looking after a few day, and is impossible to remove, or mask.Thanks for your help!! Much appreciated




Thanks for the extra info! Do you mix your resin by hand or by machine? do you use the 2-cup mixing system where you mix in the first cup then transfer everything in the second cup and mix again? this is the safest way to ensure proper mixing. Is your resin stored in the same room as where you pour it? moving your resin from a warm place to a cold place or the way might cause that skin on top. 


Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




Randy Mugford
R
Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)
Group: Forum Members
Posts: 7, Visits: 23
Matthieu Libeert - 2/6/2019 7:29:01 PM
Randy Mugford - 2/6/2019 7:19:42 PM
Matthieu Libeert - 2/6/2019 7:05:35 PM
Randy Mugford - 2/4/2019 9:32:30 PM
Lester Populaire - 2/4/2019 9:24:19 PM
Randy Mugford - 2/4/2019 6:42:41 PM
Rich (Staff) - 2/4/2019 5:35:01 PM
Hi Randy, the concept of the table looks great and you should be able to get a perfect/flawless finish so we'd like you to get to the bottom of the cause of this problem. In the first instance, what type of plastic/material are you using as the mould surface? Does it self-release (like Polypropylene) or do you use a release agent; if you use a release agent, what type are you using?

Thanks for the reply. No release agent is being used. I cast it on a very dense Polypropylene, almost glass finish. Releases easy. I apply on coat 1/4 inch thick, then after 12 hours place the wood structure in it, and pour 3 more coats each at about 1/2 inch. I never noticed it originally while pouring it, but after the job was complete the white scales started to show up and got more noticeable over time. Initially I thought it could be too much moisture, but the temp is at 22 and the moisture is very low. I noticed today after an initial pour of i/4 inch i had a film develop on about 20% of the surface ( only detectable at a certain angle) that was almost at a tacky stage after 10 minutes. I used a flat blade and removed the film, which them turned milky, and disposed of it. Problem is I cannot do this after I place the wood in. The eventual top side of the furniture piece has been and likely again will be flawless, it is the back side where the issue is, which is the side i am pour each layer on, as a result of doing the piece upside down.


That looks like amine blush type thing to me. I'd bet it is due to measuring inaccuracy or not well mixed resin. Big quantities can be hard to mix properly. 

Thank you. I will double my mix time and see what happens. I thought amine blush was a moisture reaction. I wondered if the heat gun caused the reaction. Once again thanks!

As above I would say moist related or temperature changes, unproper mixing, and now that you talk about heat gun, there is a big chance you "burned" your epoxy, if you leave your heatgun to long on a spot it will create a thin dull film. Could it also be that your wood is not completely dry? When I make my tables I leave the wood in an oven for over a week to remove any moist in the wood that might transfer into your resin when the resin goes exothermal and creates big temperatures causing the moist to "vape" into your resin causing bubbles and haze. 

Thanks. I'll put this in point form to make it quicker ...
A.  The wood is kiln dried laminate, and has 4 coats water base finish (this haze is apparent without contacting the wood). B. With or without the heat gun, same effect. C. It is mixed for 10 plus minutes, in a clear container to insure proper mixing. About three cups mixed at a time, to lesson improper mixing. Room set at 22 degrees, humidity at 40%. The haze is immediately after pouring on about 25 % of the surface, and it is random. The surface area is 12 square feet, and the resin barely contacts the wood. The haze happens within the first minute. It is only noticeable a an angle with the the right light direction. I have learned after 15 pours now to lightly scrap it off after each pour . When you scrap it it immediately developed with strands, with micro bubbles in it. I basically scrap it to the edges now and remove it. Over 12 square feet it is a hassle. If I do not remove it, it becomes white -ish and scally looking after a few day, and is impossible to remove, or mask.Thanks for your help!! Much appreciated




Thanks for the extra info! Do you mix your resin by hand or by machine? do you use the 2-cup mixing system where you mix in the first cup then transfer everything in the second cup and mix again? this is the safest way to ensure proper mixing. Is your resin stored in the same room as where you pour it? moving your resin from a warm place to a cold place or the way might cause that skin on top. 

By hand with a metal stir stick. I have not done a double cup transfer, but will try that in a few hours as I do another pour. Resin is stored in the same room as casting. If I can I will take an image later today when I do the pour and scrap the haze off. Unless of course it does not happen. Thanks againSmile

Matthieu Libeert
Matthieu Libeert
Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
Randy Mugford - 2/6/2019 7:34:58 PM
Matthieu Libeert - 2/6/2019 7:29:01 PM
Randy Mugford - 2/6/2019 7:19:42 PM
Matthieu Libeert - 2/6/2019 7:05:35 PM
Randy Mugford - 2/4/2019 9:32:30 PM
Lester Populaire - 2/4/2019 9:24:19 PM
Randy Mugford - 2/4/2019 6:42:41 PM
Rich (Staff) - 2/4/2019 5:35:01 PM
Hi Randy, the concept of the table looks great and you should be able to get a perfect/flawless finish so we'd like you to get to the bottom of the cause of this problem. In the first instance, what type of plastic/material are you using as the mould surface? Does it self-release (like Polypropylene) or do you use a release agent; if you use a release agent, what type are you using?

Thanks for the reply. No release agent is being used. I cast it on a very dense Polypropylene, almost glass finish. Releases easy. I apply on coat 1/4 inch thick, then after 12 hours place the wood structure in it, and pour 3 more coats each at about 1/2 inch. I never noticed it originally while pouring it, but after the job was complete the white scales started to show up and got more noticeable over time. Initially I thought it could be too much moisture, but the temp is at 22 and the moisture is very low. I noticed today after an initial pour of i/4 inch i had a film develop on about 20% of the surface ( only detectable at a certain angle) that was almost at a tacky stage after 10 minutes. I used a flat blade and removed the film, which them turned milky, and disposed of it. Problem is I cannot do this after I place the wood in. The eventual top side of the furniture piece has been and likely again will be flawless, it is the back side where the issue is, which is the side i am pour each layer on, as a result of doing the piece upside down.


That looks like amine blush type thing to me. I'd bet it is due to measuring inaccuracy or not well mixed resin. Big quantities can be hard to mix properly. 

Thank you. I will double my mix time and see what happens. I thought amine blush was a moisture reaction. I wondered if the heat gun caused the reaction. Once again thanks!

As above I would say moist related or temperature changes, unproper mixing, and now that you talk about heat gun, there is a big chance you "burned" your epoxy, if you leave your heatgun to long on a spot it will create a thin dull film. Could it also be that your wood is not completely dry? When I make my tables I leave the wood in an oven for over a week to remove any moist in the wood that might transfer into your resin when the resin goes exothermal and creates big temperatures causing the moist to "vape" into your resin causing bubbles and haze. 

Thanks. I'll put this in point form to make it quicker ...
A.  The wood is kiln dried laminate, and has 4 coats water base finish (this haze is apparent without contacting the wood). B. With or without the heat gun, same effect. C. It is mixed for 10 plus minutes, in a clear container to insure proper mixing. About three cups mixed at a time, to lesson improper mixing. Room set at 22 degrees, humidity at 40%. The haze is immediately after pouring on about 25 % of the surface, and it is random. The surface area is 12 square feet, and the resin barely contacts the wood. The haze happens within the first minute. It is only noticeable a an angle with the the right light direction. I have learned after 15 pours now to lightly scrap it off after each pour . When you scrap it it immediately developed with strands, with micro bubbles in it. I basically scrap it to the edges now and remove it. Over 12 square feet it is a hassle. If I do not remove it, it becomes white -ish and scally looking after a few day, and is impossible to remove, or mask.Thanks for your help!! Much appreciated




Thanks for the extra info! Do you mix your resin by hand or by machine? do you use the 2-cup mixing system where you mix in the first cup then transfer everything in the second cup and mix again? this is the safest way to ensure proper mixing. Is your resin stored in the same room as where you pour it? moving your resin from a warm place to a cold place or the way might cause that skin on top. 

By hand with a metal stir stick. I have not done a double cup transfer, but will try that in a few hours as I do another pour. Resin is stored in the same room as casting. If I can I will take an image later today when I do the pour and scrap the haze off. Unless of course it does not happen. Thanks againSmile

hope it wont happen but if it does share some pictures Smile visuals are always easier to find answers BigGrin


Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




Randy Mugford
R
Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)Forum Guru (54 reputation)
Group: Forum Members
Posts: 7, Visits: 23
Matthieu Libeert - 2/6/2019 7:58:52 PM
Randy Mugford - 2/6/2019 7:34:58 PM
Matthieu Libeert - 2/6/2019 7:29:01 PM
Randy Mugford - 2/6/2019 7:19:42 PM
Matthieu Libeert - 2/6/2019 7:05:35 PM
Randy Mugford - 2/4/2019 9:32:30 PM
Lester Populaire - 2/4/2019 9:24:19 PM
Randy Mugford - 2/4/2019 6:42:41 PM
Rich (Staff) - 2/4/2019 5:35:01 PM
Hi Randy, the concept of the table looks great and you should be able to get a perfect/flawless finish so we'd like you to get to the bottom of the cause of this problem. In the first instance, what type of plastic/material are you using as the mould surface? Does it self-release (like Polypropylene) or do you use a release agent; if you use a release agent, what type are you using?

Thanks for the reply. No release agent is being used. I cast it on a very dense Polypropylene, almost glass finish. Releases easy. I apply on coat 1/4 inch thick, then after 12 hours place the wood structure in it, and pour 3 more coats each at about 1/2 inch. I never noticed it originally while pouring it, but after the job was complete the white scales started to show up and got more noticeable over time. Initially I thought it could be too much moisture, but the temp is at 22 and the moisture is very low. I noticed today after an initial pour of i/4 inch i had a film develop on about 20% of the surface ( only detectable at a certain angle) that was almost at a tacky stage after 10 minutes. I used a flat blade and removed the film, which them turned milky, and disposed of it. Problem is I cannot do this after I place the wood in. The eventual top side of the furniture piece has been and likely again will be flawless, it is the back side where the issue is, which is the side i am pour each layer on, as a result of doing the piece upside down.


That looks like amine blush type thing to me. I'd bet it is due to measuring inaccuracy or not well mixed resin. Big quantities can be hard to mix properly. 

Thank you. I will double my mix time and see what happens. I thought amine blush was a moisture reaction. I wondered if the heat gun caused the reaction. Once again thanks!

As above I would say moist related or temperature changes, unproper mixing, and now that you talk about heat gun, there is a big chance you "burned" your epoxy, if you leave your heatgun to long on a spot it will create a thin dull film. Could it also be that your wood is not completely dry? When I make my tables I leave the wood in an oven for over a week to remove any moist in the wood that might transfer into your resin when the resin goes exothermal and creates big temperatures causing the moist to "vape" into your resin causing bubbles and haze. 

Thanks. I'll put this in point form to make it quicker ...
A.  The wood is kiln dried laminate, and has 4 coats water base finish (this haze is apparent without contacting the wood). B. With or without the heat gun, same effect. C. It is mixed for 10 plus minutes, in a clear container to insure proper mixing. About three cups mixed at a time, to lesson improper mixing. Room set at 22 degrees, humidity at 40%. The haze is immediately after pouring on about 25 % of the surface, and it is random. The surface area is 12 square feet, and the resin barely contacts the wood. The haze happens within the first minute. It is only noticeable a an angle with the the right light direction. I have learned after 15 pours now to lightly scrap it off after each pour . When you scrap it it immediately developed with strands, with micro bubbles in it. I basically scrap it to the edges now and remove it. Over 12 square feet it is a hassle. If I do not remove it, it becomes white -ish and scally looking after a few day, and is impossible to remove, or mask.Thanks for your help!! Much appreciated




Thanks for the extra info! Do you mix your resin by hand or by machine? do you use the 2-cup mixing system where you mix in the first cup then transfer everything in the second cup and mix again? this is the safest way to ensure proper mixing. Is your resin stored in the same room as where you pour it? moving your resin from a warm place to a cold place or the way might cause that skin on top. 

By hand with a metal stir stick. I have not done a double cup transfer, but will try that in a few hours as I do another pour. Resin is stored in the same room as casting. If I can I will take an image later today when I do the pour and scrap the haze off. Unless of course it does not happen. Thanks againSmile

hope it wont happen but if it does share some pictures Smile visuals are always easier to find answers BigGrin
The camera could not catch it properly, however you can see that once scrapping the film off, it clumps together and is white. this happens with 1 minute for the pourSad



GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Randy Mugford - 6 Years Ago
Rich (Staff) - 6 Years Ago
Randy Mugford - 6 Years Ago
SleepingAwake - 6 Years Ago
Randy Mugford - 6 Years Ago
matthieutje65 - 6 Years Ago
Randy Mugford - 6 Years Ago
matthieutje65 - 6 Years Ago
Randy Mugford - 6 Years Ago
                                         hope it wont happen but if it does share some pictures :) visuals are always easier to find answers :D
matthieutje65 - 6 Years Ago
Randy Mugford - 6 Years Ago
Warren (Staff) - 6 Years Ago
Randy Mugford - 6 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search