Group: Administrators
Posts: 167,
Visits: 4.6K
|
Hi John, Can I just check; is this GlassCast (You've put Clear Cast) so want to ensure we're talking about the same product; if so, the mix ratio when mixing by weight is 100:45 rather than 2:1, the latter is the ratio when measuring by volume; its worth checking as getting it the wrong way round can give some curing issues.
What temperatures are you working in and what temperature is the resin when you're mixing it? At lower temps, the viscosity increases quite significantly and when it is thicker, it struggles to release air as easily; to avoid this, ensure that both your environment and the resin itself is at least 20'C as this should ensure it naturally degasses without a problem.
|