Hi,
It's long time since I have wrote anything and I wanted to share some of my experiences now. 

As many of U may know, I have been working with carbon fiber and fiberglass parts for a long time. Mostly every composite part that I have been making, is made by resin infusion. Problem with resin infusion have been always the fact that sealing the vacuum bag takes a lot of time and it is very easy leave it to have a leak. As I have wrote in some older thread, the micron meter helped a lot to get reliable sealing. Basic vacuum gauges are not enough to determine 100% reliable that is the bag leaking or not(unless u wait long time and check vacuum drop). Since we need to make so many parts and we need a fast cycle for the parts we have been going more and more to reusable silicon bags. Basically we no longer make basic resin infusion with nylon bags. There is several reasons for it:

-Silicon bag is reusable (some companies have used it for cycle of 3000)
- No Waste
- 100% reliable sealing (never vacuum leaks)
- Can hold vacuum for days without running vacuum pump
- Seals in matter of seconds
- Made in the shape of the mould, so there will be no corners that the bag wont be reaching.
- Environmentally friendly.

Of course it's a investment to make the silicon vacuum bag, so its not good for one off items, but if u make more than 2 parts, it will definitely be worth of making it. Negative thing of the bag is that it wont be lasting for long with epoxy parts. Lifetime will be 25-100 cycles. I made a 1,3 meter long miniature boat hull mould with silicon bag for demo purpose and it took just minutes to infuse the part. After I have add the fiberglass, I just add the silicon bag over it and I will get perfect vacuum in matter of seconds and its ready for infuse. I never had any leaking issues with the silicone bag. Also with a Morph runner I can make a channel for resin flow, that after infusion I am able to get it disappear. No traces of flow channel, so no need for removing hardened resin, like normal channels would leave. 

I am not promoting anything or selling anything with this text. I just want to give u all my honest opinion of silicon vacuum bags. Highly recommend for testing it. Smile


Reply
Finnluxury
Finnluxury
Supreme Being (345 reputation)Supreme Being (345 reputation)Supreme Being (345 reputation)Supreme Being (345 reputation)Supreme Being (345 reputation)Supreme Being (345 reputation)Supreme Being (345 reputation)Supreme Being (345 reputation)Supreme Being (345 reputation)
Group: Forum Members
Posts: 50, Visits: 448
Hi Warren. I would recommend to go Alan Harper workshops. Or ask Blaise from Alan Harper to visit your company. They are super friendly and very professional with silicone bags. I think it would be good idea for Easy Composites to start selling the silicone that Alan Harper provides. Its quite simple to make the bags, when U see how it works. 

Hanaldo, I can send U some pictures later on. I have silicone square profile that I use to make the channel and after mould is ready, I change it to round one to get perfect finish. Are U doing the same way? Both ends of the silicone profile must end to the outer vacuum channel of the bag, This prevent any vacuum leakage to happen. 

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Finnluxury - 7 Years Ago
Hanaldo - 7 Years Ago
Finnluxury - 7 Years Ago
SleepingAwake - 7 Years Ago
Hanaldo - 7 Years Ago
Warren (Staff) - 7 Years Ago
scottracing - 7 Years Ago
Finnluxury - 7 Years Ago
Dezer - 7 Years Ago
scottracing - 7 Years Ago
Dezer - 7 Years Ago
SHaas - 7 Years Ago
scottracing - 7 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search