The basic principle is the same except that expansion and contraction due to the heat cycle are very important here. Ideally you need to minimise or take into account the difference in CTE of the mould and part.
Imagine your mould above in aluminium, the aluminium and carbon would expand as it is heated, then the carbon cures and the heat is turned off. As the temperature drops, the aluminium will contract more than the carbon meaning the inner mould will probably self release but the outer mould will grip the part making the release very hard if not impossible. With a composite mould, for example, that issue would be significantly reduced. You could tweak the mould design to aid release and take this into account.