Group: Forum Members
Posts: 2.5K,
Visits: 28K
|
Post cure means exposing the part to elevated temperatures for a period of time, eg. 60 degrees C for 16 hours.
It is fairly likely you don't have an oven to do the post cure in, so you can either get a set of 500W halogen work lights and position them on the parts for 8 hours over 2 days, or you can leave the car sitting out in direct sunlight for a few days. Trouble with leaving it in the sun is if it then gets hotter later in the year than it is now, then you will likely go over the resins temperature capabilities again and have to repeat the process. So it's always best to try and get the parts as close to the maximum Tg of the resin as you can.
|