Why would UD appear dry after vac bagging?


Author
Message
flanagaj
flanagaj
Junior Member (22 reputation)Junior Member (22 reputation)Junior Member (22 reputation)Junior Member (22 reputation)Junior Member (22 reputation)Junior Member (22 reputation)Junior Member (22 reputation)Junior Member (22 reputation)Junior Member (22 reputation)
Group: Forum Members
Posts: 2, Visits: 10
I have just vac bagged 2 layers of UD onto the top of my bike frame, but when I debagged the frame, the UD appears as though it does not contain any resin and when I tried sanding it, it sort of sanded, but was quite stringy (hope that makes sense).  

I thoroughly wetted out the 2 layers and also ensured the peel ply was wetted out that I put on top of the UD, but I did forget to put a layer of release film between the peel ply and the breather fabricl.  Would the breather material have soaked up all of the resin and caused the problem I mention?

Thanks

polaraligned
polaraligned
Supreme Being (188 reputation)Supreme Being (188 reputation)Supreme Being (188 reputation)Supreme Being (188 reputation)Supreme Being (188 reputation)Supreme Being (188 reputation)Supreme Being (188 reputation)Supreme Being (188 reputation)Supreme Being (188 reputation)
Group: Forum Members
Posts: 13, Visits: 284
flanagaj (27/03/2017)
I did forget to put a layer of release film between the peel ply and the breather fabricl.  Would the breather material have soaked up all of the resin and caused the problem I mention?





Yup. The breather soaked it up. 

Edited 9 Years Ago by polaraligned
Rich (Staff)
Rich (Staff)
Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)
Group: Administrators
Posts: 167, Visits: 4.6K
The breather will certainly have soaked up the resin - it in effect acts like a sponge; with a perforated release film and 20-25% vacuum level, you should restrict the amount soaked up only to any excess applied whilst laminating.
flanagaj
flanagaj
Junior Member (22 reputation)Junior Member (22 reputation)Junior Member (22 reputation)Junior Member (22 reputation)Junior Member (22 reputation)Junior Member (22 reputation)Junior Member (22 reputation)Junior Member (22 reputation)Junior Member (22 reputation)
Group: Forum Members
Posts: 2, Visits: 10
Rich (Staff) (28/03/2017)
The breather will certainly have soaked up the resin - it in effect acts like a sponge; with a perforated release film and 20-25% vacuum level, you should restrict the amount soaked up only to any excess applied whilst laminating.


Ok Thanks.  I'll give it another shot with release film and reduced vacuum.
GO