HI Zymka,
Have you tried without the Styrene? I suspect thinning down the GC50 has meant that during the cure it has pulled from the surface a bit more perhaps shrinking back a bit more as the extra styrene evaporates off during the cure. Also the GC50 is typically the correct viscosity for spraying onto a mould so thinning it down may have reduced the surface tension of the gel making it more prone to pull away from the surface like you have seen as it cures.
We do not recommend thinning of GC50 with styrene in the majority of cases.
Warren Penalver Easy Composites / Carbon Mods - Technical Support Assistant
|