Take it in gradual steps for example, 2 hours at 20C, 2 hours at 40C, 2 hours at 60C and then say 6 hours at 80C then allow to cool naturally. That should bring you upto 80C. You have to do small steps when postcuring rather than just jumping to a high temperature because you are trying to avoid the resin softening (which is what causes the print through in your case it seems).
Warren Penalver Easy Composites / Carbon Mods - Technical Support Assistant
|
|
|
|
|
thanasiss3
|
|
|
Group: Forum Members
Posts: 18,
Visits: 348
|
The guy at the shop tell me to slowly raise the temperature and stay at the target temperature for a few hours,he didnt seem to know a tds,i found at the web some pdfs for the megapoxy 132(epoxy that i use)and they not say anything. So i must try and error,first attemp was heat for 8 hours at 65-75 celcius,i cant heat very much cause the cores are abs plastic If the epoxy layer is really thick the print through will be eliminate?
|
|
|
|
|
Warren (Staff)
|
|
|
Group: Administrators
Posts: 2.5K,
Visits: 8.5K
|
In the hot sun dark coloured interior parts can get above 60C. The average pain threshold for temperature for most humans is around 54C yet even here in the "sunny" UK it is common on a hot day to find it initially painful to sit on or touch black leather interior trims or metal gearknobs
You will find most effective post cures will go upto or very close to the target heat distortion temperature. So if you want to achieve a 140C Tg on your resin (if it is suitable of course) then your post cure will likely hit at least 120C.
Your resin manufacturer should be able to give you a postcure schedule for the resin system.
Warren Penalver Easy Composites / Carbon Mods - Technical Support Assistant
|
|
|
|
|
thanasiss3
|
|
|
Group: Forum Members
Posts: 18,
Visits: 348
|
What Tg supposed to be effective for interior parts?hot greek sun can touch 40-45+ at a sunny day! The megapoxy i use refere as working temp 50without postcure and 140with the appropriate postcuring! I hope the post curing profile i use can have a good Tg! Thiw epoxy has great clearance!!!
|
|
|
|
|
Hanaldo
|
|
|
Group: Forum Members
Posts: 2.5K,
Visits: 28K
|
Clear coat won't prevent print through if it does reoccur though. If the post-cure doesn't help, you may have to consider switching to a higher Tg resin system.
|
|
|
|
|
thanasiss3
|
|
|
Group: Forum Members
Posts: 18,
Visits: 348
|
I let the laminated parts to cool down,they get again rock hard,the clearance of epoxy is at higher levels,the abs plastic core get hard again! The surface get the print trough,so there is a need to wet sand smooth and clearcoat!
|
|
|
|
|
Hanaldo
|
|
|
Group: Forum Members
Posts: 2.5K,
Visits: 28K
|
You need to let it cool down again yes. This may take a bit of experimentation without the TDS, as it's possible that 75 is just too far above your resins Tg and it could be degrading the resin. Don't forget a nice yet though, you need to let the part cool back down to ambient temperature before you debag.
|
|
|
|
|
thanasiss3
|
|
|
Group: Forum Members
Posts: 18,
Visits: 348
|
I backe the parts at an oven with elevated temperature,2hours at 40,2 hours at 60 and 2 hours at 75,after the cycle,the parts ofcourse get warm and epoxy get soft,you can hit them with your nail,is it ok or did something wrong? When they cool down,will it get rock hard?
|
|
|
|
|
Dravis
|
|
|
Group: Forum Members
Posts: 592,
Visits: 1.9K
|
Its almost always a "stepped" post-cure cycle .. 2 hours at 40, 2 Hours at 60, 2 hours at 80 ... etc. Doing something like that will never damage the parts, and will almost certainly improve them.
"Sapere Aude"... Dare to KNOW!
The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...
103% of all people do not understand statistics...
Do not adjust our mind, theres a fault in reality :-)
|
|
|
|
|
thanasiss3
|
|
|
Group: Forum Members
Posts: 18,
Visits: 348
|
I use megapoxy 132,the tds is not availiable,the shop where i bought it said it can withstand temperature over 130degrees if post cured,but they not give me extra information
|
|
|
|