Well ... the specs say that it will remain bondable "for up to 24 hours" --
I have sucessfully infused parts more than 24 hours after spraying GC50, but I knew ahead that I would not be able to make it in the 24 hours, so after around 2 hours at 20 Deg in my workshop, I stored the parts in my garage, which at that time was around 10 deg. C.
The next day I brought them back to my workshop, and set up all the infusion kit, and bagged it. that took around 25 mins ..
I infused, and the parts were fine. I used one of them for a "Destructive test" along with other parts of similar "build" and the 24 hour+ parts were just as strong as the others, and did not delaminate more than the standard parts ..