Hello!

First hi to everyone using this forum, you got nice community here.

Ok the PROBLEM Smile

I am using 245 2x2 twill 43% resin rich prepreg. As you can see the resin in not equally spread through surface.

http://www.talkcomposites.com/Uploads/Images/a746b9e6-2ca7-466c-979d-6ad2.jpg

My product demands 2 layers of prepreg so when i stack the layers i turn the the sides with more resin facing each other then i combine them so the most resin is in the middle of fibres letting the vacuum do its job.

When i vacuume the prepreg i use release film perforated and breather all stuck in vacuumbag.

 
My tactic is 3h of vacuuming on room temp then 1-2h on 45C, 1h on 60C and 1h on 70C after that i cure it at 120C for another hour more

This is my BEST result :
http://www.talkcomposites.com/Uploads/Images/776ae16c-55ea-4f41-813b-0564.jpg http://www.talkcomposites.com/Uploads/Images/548b377e-f518-4eb1-8898-4353.jpg

So here is the problem why is here areas of pinhole free surface and with pinholes is it the resin not evenly spread the or the problem is my tactic of vacuuming any tips or help will be nice.

P.S. I am using http://shop1.r-g.de/item/390102S  vacuum pump 



Edited 11 Years Ago by primoz1111
Replies
primoz1111
primoz1111
Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)
Group: Forum Members
Posts: 3, Visits: 31
Hello!

Tnx for all replays. 

It was help full ALLOT!!! i did it no pinholes at all i cant be more happy.

http://www.talkcomposites.com/Uploads/Images/0de77f65-a57f-4497-bd68-b68a.jpg

Tnx for all yours hellp!!
creator
creator
Supreme Being (83 reputation)Supreme Being (83 reputation)Supreme Being (83 reputation)Supreme Being (83 reputation)Supreme Being (83 reputation)Supreme Being (83 reputation)Supreme Being (83 reputation)Supreme Being (83 reputation)Supreme Being (83 reputation)
Group: Forum Members
Posts: 9, Visits: 92
primoz1111 (22/04/2015)
Hello!

Tnx for all replays. 

It was help full ALLOT!!! i did it no pinholes at all i cant be more happy.

http://www.talkcomposites.com/Uploads/Images/0de77f65-a57f-4497-bd68-b68a.jpg

Tnx for all yours hellp!!

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...





Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search