Hi all

I want to try infusing a part with a partial in-mould coating of gelcoat, so that only a selected strip of the carbon fabric is visible within a part largely showing a coloured gelcoat surface finish

However, when using the spray gun and masking off the edges of moulds using normal masking tape it hardly sticks at all on moulds that are well treated with Easylease

Is there a better tape out there that will provide a bit more tack whilst not compromising the release coated surface? Not sure if there is a real danger of the release agent being 'pulled away' by the tape adhesive?

Also, has anyone found a reliable timeframe in which to remove the tape without pulling away the coating or ruining the sharpness of the masked lines?

Cheers
kidpaint
kidpaint
Supreme Being (778 reputation)Supreme Being (778 reputation)Supreme Being (778 reputation)Supreme Being (778 reputation)Supreme Being (778 reputation)Supreme Being (778 reputation)Supreme Being (778 reputation)Supreme Being (778 reputation)Supreme Being (778 reputation)
Group: Forum Members
Posts: 99, Visits: 676
Can you just infuse the part without the gel coat and once done, mask off the part and paint it? 
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Best bet is to do 3 or 4 coats of release wax over the top of the Easylease. Should raise the surface tension enough for the masking tape to stick. You do still need to be careful though, you can blow the tape off with the spray gun if you get too close or give it too much pressure. It could well take you a couple of tries before you get it right. 
The Fibreglass King
The Fibreglass King
Supreme Being (501 reputation)Supreme Being (501 reputation)Supreme Being (501 reputation)Supreme Being (501 reputation)Supreme Being (501 reputation)Supreme Being (501 reputation)Supreme Being (501 reputation)Supreme Being (501 reputation)Supreme Being (501 reputation)
Group: Forum Members
Posts: 69, Visits: 652
Hello Mark,
The best tape to use is 3m fine line. Make sure you seal the tape to your mould by rubbing the edge of the tape to the mould surface, once  the gel has been applied pull the tape towards the gel to get a nice crisp line.
Kind Regards
The Fibreglass King
MarkMK
MarkMK
Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)
Group: Forum Members
Posts: 338, Visits: 2K
Thanks for the replies. I'll give the 3M a go along with the addition of some wax coats and prepare myself for a bit of experimentation with regards to timing. Painting afterwards would indeed appear the most straightforward option and one I might resort to ifall else fails Smile
MarkMK
MarkMK
Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)
Group: Forum Members
Posts: 338, Visits: 2K
Just as an update on this, I used the 3m tape as recommended and it worked great. Very nervy pulling the tape away and I only left it for half an hour as didn't want to risk a big sections of partially cured gelcoat coming away
  
Attached are a couple of pics showing the masked off mould (I framed two pieces of bagging film first with the tape first with enough of a lip to stick down) and the final part

I didn't manage to exactly match the pigment and the choice of fabric was probably wrong but as a test of what's possible it was worth it. 
Attachments
20150519_162242.jpg (827 views, 1.00 MB)
20150527_142205.jpg (794 views, 2.00 MB)
20_rc51_00
20_rc51_00
Supreme Being (685 reputation)Supreme Being (685 reputation)Supreme Being (685 reputation)Supreme Being (685 reputation)Supreme Being (685 reputation)Supreme Being (685 reputation)Supreme Being (685 reputation)Supreme Being (685 reputation)Supreme Being (685 reputation)
Group: Forum Members
Posts: 95, Visits: 548
Great! THanks for the follow up! Nice job!
Fasta
Fasta
Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)
Group: Forum Members
Posts: 468, Visits: 3.5K
That looks great, have you got a pic of the whole car/bike?







The Fibreglass King
The Fibreglass King
Supreme Being (501 reputation)Supreme Being (501 reputation)Supreme Being (501 reputation)Supreme Being (501 reputation)Supreme Being (501 reputation)Supreme Being (501 reputation)Supreme Being (501 reputation)Supreme Being (501 reputation)Supreme Being (501 reputation)
Group: Forum Members
Posts: 69, Visits: 652
Hello Mark,
                     That does look neat!, well done on a tidy job! I think a decrotive red and black carbon with a smaller weave would look smart.....??
Kind regards
The Fibreglass King....
MarkMK
MarkMK
Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)
Group: Forum Members
Posts: 338, Visits: 2K
Thanks for the positive comments gents

The process seemed  to work well. However, some friends with similar cars were a bit 'lukewarm' to the idea. One commented that it looked a bit like someone had stuck some vinyl wrap to a GRP wing! The slightly different choice of fabric didn't seem too well received either (heathens!).

I've stuck with good old twill weave for now, but might return to the idea later and yes, it might work better using different fabric and perhaps trying some of the hybrids is the way to go

I've attached some pics of the whole car which has some bits on I've recently made, including side panels, half-doors, diffuser, boot panel and aero screen. The front cycle wings, pictured separately, have been modified from an item more widely available to include a ducted section. The practical purpose is to release air from underneath and reduce any 'lift' at speed, but if I'm honest it's probably more of a cosmetic mod Smile. Believe it or not, each wing has eight separate pieces of carbon making up the surface layer. A bit fiddly, but you really can hide most of the joins in the curves (aside from the side profile where it's nigh on impossible to get  the weave to match the top surface all the way round in an acceptable manner).







Edited 11 Years Ago by MarkMK
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search