Hi, my wife has a full carbon Allwave Vanguard Outrigger canoe.

It is only about 12 months old and we have just removed the cover after being stored for the winter to find an extensive 'roughness' on the gel coat - like tiny bubbles, really course to the touch. Also in places, there is visible bubbling, see picture.

She has only over used plain water to clean it (after ever use) and 'Car Plan bumper shine' to polish it, which was recommended by the seller.
It has been stored in a nylon sock and not come into contact with any chemicals. There was no problem when it was last used in October/early November - could frost have damaged it?

Firstly, can you suggest what might have caused the problem, and secondly what products do I need to repair it. I specifically want to know if I need to colour the gel coat (the boat has a multi-colour design!!) or will I be able to just sand away the bubbles and re-coat it with clear gel.

http://www.talkcomposites.com/Uploads/Images/72351c7a-f577-4d35-8090-1824.jpg
(The darker lines are reflection of trees)
Replies
ChrisR
ChrisR
Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)
Group: Forum Members
Posts: 363, Visits: 3K
I've had this before, it looks like early osmosis but it maybe something else unknown.

Points of note:
1) Dry it out - really dry it out i.e. stick it in the house (heated space) for a month or two, but before hand using a very soft pencil (4B or china pencil) mark around the bubbles. you may find most of them just go away - then you can either fix the areas or just leave them be and rub off the pencil markigns.
2) Is it actually gelcoat? If it's a full CF canoe then it may just be a mould or post applied paint - If thats the case then it may just be contamination causing the bubbles
3) Don't store it enclosed outside i.e. in a sock where some dampness can remain, if you intend to leave it outside make sure it's fully ventilated.

How do I know this? I stored my boat in a workshop for a few years without using it - the place get damp and wasn't well vented, osmosis bubbles came up everywhere, I changed the storage location to a fully vented barn and they all went away
flash68
flash68
Forum Member (45 reputation)Forum Member (45 reputation)Forum Member (45 reputation)Forum Member (45 reputation)Forum Member (45 reputation)Forum Member (45 reputation)Forum Member (45 reputation)Forum Member (45 reputation)Forum Member (45 reputation)
Group: Forum Members
Posts: 7, Visits: 67
Thanks for your replies,

ChrisR, unfortunately bringing it indoors is not an option being 7.5m (23ft) long, although I am trying to find a secure barn or such like to rent some space, so I may have to wait for the warmer weather for it to dry out properly.

Since my first post I've noticed that the bubbling is not around the open cockpit area but only around each of the bulkheads, which are sealed except for a small bung. Removing the bung revealed that both bulkheads are very wet inside (although no water seems to be flowing around in them), but there is crystalised salt inside - the previous owner used the boat on the sea. I'm leaving the bungs out but they are very small so will take a long time to dry out, would it be better to wash them out with fresh water first or just leave them to dry?

Interesting what you say about not storing it in a sock - it has been stored outside on tressles, upside down so water has not collected in it, but the nylon sock has been repeatedly wet and dried with the weather, so I this wont have helped. I will do as you suggest and remove the sock and if I can't get storage I will make something like an open ended poly-tunnel.

Warren, how easy is it to match the colour (white)?
Edited 10 Years Ago by flash68
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
flash68 - 10 Years Ago
panda - 10 Years Ago
flash68 - 10 Years Ago
Warren (Staff) - 10 Years Ago
ChrisR - 10 Years Ago
flash68 - 10 Years Ago
dbcrx - 10 Years Ago
flash68 - 10 Years Ago
carbonfibreworks - 10 Years Ago
flash68 - 10 Years Ago
dbcrx - 10 Years Ago
Dravis - 10 Years Ago
flash68 - 10 Years Ago
panda - 10 Years Ago
flash68 - 10 Years Ago