What size batches are you mixing? ideally it needs to be within 1%. It could be quite easy to be a few % out.
Adding extra hardener will never work with epoxies as the chemistry is such that there needs to be a precise amount of each part to react with each other. As such adding extra hardener will make things worse almost gauranteeing a tacky finish.
The rapid repair at a constand 25C should be hard within a couple hours at most. It is possible that your environment is still quite humid and that would effect the cure. However normally you see excessive humidity as a slight milkyness in the resin.
It is normal for an epoxy to soften on first application of heat. This is because at room temperature it does not fully cure initially so the application of heat softens it.
Warren Penalver Easy Composites / Carbon Mods - Technical Support Assistant
|