			            I divide my total resin requirement into 400-500 grm batches. I find I can mix those amounts without introducing too much air. 
  What is important is that your resin is at 20 degrees C minimum. If you have an oven put the resin container in there whilst your bagging up to bring it up to temperature. If not at least bring the resin into the house the night before. And the mould if your workshop is particularly cold.
  Decant the total resin requirements into equal amounts, add hardener to the first batch and mix. Start the infusion but don't open the line clamp fully. Once you get a feel for the resin uptake start mixing the second batch, adjust the line clamp so that you wont run out before the second batch is ready. You will soon get a feel for it and find a setting that suits. When adding resin to the first pot poor it slowly down the side of the pot, this way you shouldn't add air into the mix. Continue mixing/adding until the infusion is complete. 
  As soon as you start mixing large batches of resin the clock is ticking, chances are on a new mould/layup with unknown flow rates the resin in the pot will begin to gel long before the infusion is complete. This is one of the many reasons I prefer infusion, you have much greater control.
  Hope that makes sense. Warren                
			            
  				