Group: Forum Members
Posts: 237,
Visits: 4.8K
|
Did you post cure your mould before you put the release on for the pre preg ?
You need to burn the styrene out,if not when you cure the styrene comes out on your first cure taking your release with it
Normal household oven is ok to cure for a cure on a item like this but if you were to do another you really need a separate internal bag joined onto your outer bag rather than trying to push your outer bag down into the mould
|