			            Hey Turbo, as I was saying, I like to slow my resin inlet (by slowly opening the resin clamp on the feed line and bleeding it in), to ensure that everything is wet out. You place the mti hose around the perimeter of the mould (I would go all around the mould on this one) probably need 2-3 meters of hose. The resin has plenty of time to reach alllll corners of the mould and wet out everything before it gels, depending on what resin you are using. My pot life is by far long enough to degass the resin thoroughly and infuse slowly. 
  The MTI is designed as such, that resin will reach everywhere it is placed no matter what, no need for a catch-pot either. Once you have done it several times, it becomes easier to gauge the amount of resin u need. The catch pot is placed at a 1 meter below mould elevation, which results in a very high fiber to resin ratio.                
			            				
			                                 
                     
                                            
                         
                    
                  
             |