What are you using to make the flanges? When I did the mould for my wing I used sign board. I used a piece 150mm bigger than the wing. Placed the wing centrally on the sign board, drew around it and then cut out the shape of the wing from the middle. If you cut the hole slightly undersize you can make it a tight fit over the wing. Push the sign board over the wing and position it where you want the split line. It will hold itself in place if you get the fit right. You can bend the sign board to follow the curve of the end sections. A few blobs of hot melt glue here and there, fill any gaps with filleting wax and job done. Hope that helps.