As a broad brush estimate, you will need 3-4 layers of the glass per mm of laminate. It depends obviously how well you consolidate the layers and/or use vacuum bagging or similar to compress.
In terms of resin weight, you are looking at roughly the same weight in resin as the weight of reinforcement for wet lay. Plus a little extra for mixing and wastage.