Group: Administrators
Posts: 2.5K,
Visits: 8.5K
|
It depends how important it is to accurately replicate the bonnet edges where it wont be seen once bonnet is closed.
If not important, dont worry about swage line and end the bonnet edge so that no mechanical lock can occur. If the swage is important, then you want a 3 part mould to prevent locking. Ie the sides of the bonnet have a small detachable moulding you bolt in. You then laminate within it, let it cure, unbolt the sides and the completed bonnet will come out then.
The hard part is getting the flange edge precisely in the right place for the moulding process.
Warren Penalver Easy Composites / Carbon Mods - Technical Support Assistant
|