Hello from Spain,

I've been learning about resin infusion for the last months but still find some issues I can't fully understand.

I'll try to explain what happened to my last two infusion projects and hope I can find some answers...

One of the projects was a flat sheet compossed by 1 layer of twill CF, 1 layer of matt GlassF, 1 layer of plain kevlar, 1 layer of diolen, 1 layer of matt GlassF, 1 layer of plain kevlar.

The other one was a more complex shape but only compossed by 1 layer of twill CF, some strands of CF to increase strengh in the dessired direction, 1 layer of matt Glass fiber (only in specific points to build up some thickness) 1 final layer of diolen.

Both molds were under 'full' vacuum (-1 bar gauge reading), closed inlet and vacuum ports and left for 12 hours watching fors lacks. No lacks found, pressure kept at -1bar gauge after 12 hours.

Mixed resin (EC infusion with fast hardener), degassed the resin and after a couple of minuts started infusion.

Here starts the headache...

Once the infusion started I could see air boubles travelling across the mould and the vacuum port showed air mixing with the resin while the inlet port showed cristal clear resin flowing into the mould.

This happend in both projects.

The 'full mounting'
http://www.talkcomposites.com/Uploads/Images/00b87561-4ac8-4de0-a409-ffbd.jpg

Inlet port
http://www.talkcomposites.com/Uploads/Images/214bb1cd-a780-4e93-a397-305d.jpg
Vacuum port
http://www.talkcomposites.com/Uploads/Images/9ac172f1-f70e-45fd-9e39-cb04.jpg
Trapped air
http://www.talkcomposites.com/Uploads/Images/da4aa1cb-3b6e-4a29-9782-2cc8.jpg
Final results
http://www.talkcomposites.com/Uploads/Images/8b730cf7-faa2-4804-bb68-e1e9.jpg

http://www.talkcomposites.com/Uploads/Images/b0ed849c-9d98-4e33-85c8-2b57.jpg
Air showing, this are the only cosmetical results on the final product, not a real issua as it can be solved with the laquer, but this pinholes shouldn't be there in a infusion project...any idea of what may be happening?
http://www.talkcomposites.com/Uploads/Images/8d6cd246-d80b-42fc-9cba-7d76.jpg

Thanks a lot!!
Reply
sabel
sabel
Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)Junior Member (19 reputation)
Group: Forum Members
Posts: 3, Visits: 13
Thank you all for the answers!

Job haven't left too many time to spend in my 'test lab' Tongue but I think I found what was happening.

Andy not a Temp issue this time as we are well above 30ºC Cool.

Alessandro, thanks for the idea, I'll do it from now on because I am doing small parts and the infusion is quite fast for most of them.

Well, I think the problem was the glass mat fibre. Replicated two more flat plates with different fibres but all of them woven fabric and then the infusion was perfectly smooth and with no air bubbles forming.

So, if I'm rigth... can't be mat fibres used into a infusion system? Doze