I need some help, I just recieved my first order of prepreg and after playing with it for the last couple days I am horribly disappointed.  I have been working with other prepregs from another supplier and I have had pretty good success with conventional prepreg that is meant to be cured in an autoclave even though I have been using it in an out of autoclave process.  So far the first 5 things I have tried to make with easy preg have all been complete failures.  I am super frustrated because I spent a lot of money to buy a couple yards of the material and have it sent to the US and at this point I am feeling like it all needs to be thrown in the trashcan because it seems completely useless.  I will describe the setup that I am using and maybe someone can tell me what I might be doing wrong.  I will also attach some pictures of the problems I am having.  I have tried metal molds, composite molds with a gelcoat surface, cnc machined solid teflon molds, and tonight even a sheet of glass to see if I could get a good surface finish and so far all have failed miserably.  For my mold release I am using a chemical release called Freekote 700nc which has performed beautifully with the other prepregs I have used.  I am vacuum bagging with a flexible bagging material called stretchlon 200 and with a solid release film and a breather cloth.  I have used cure schedules all over the map from 180 deg F for ten hours up to 275 deg F for less than an hour and all have yielded similar results  The max amount of vac I am able to achieve here is about 26.5inches of mercury and that has proven to be acceptable for the other prepreg I have used but I am wondering if it is not enough for the easy preg because I have read a couple of places that a near perfect vac level above 29 inches is necessary.  I leave the vac pump running throughout the process every time.  To top it all off I am not at all happy with how the cured fiber looks and  find it to be some of the most boring carbon fiber I have ever seen anywhere.  There seems to be such a lack of contrast of the alternating fibers that it almost doesn't even look like carbon fiber at all, I would hope that if I could get my surface finish issues resolved the appearance might also improve but I am skeptical that it will ever look as good as any of the other various  fabrics I have worked with.  For me the selling point of this prepreg was that it was great for making cosmetic parts and I am disappointed to say the least.  I appreciate any input that I can get and really hope that I am doing something wrong and that I can learn to love this easy preg!  Thanks for your help.

The first two pictures show a piece that I cured on glass,  It consists of one surfacing layers and two backing layers bagged up as  I have described above.  The last two pictures show some parts I have made with another brand of prepreg shown with the same piece molded on glass.  The skull and the outlet cover do have automotive clear coat on them and although I realize that it may not seem like a fair comparison I can tell you that the clear coat does not hide any flaws, but if anything tends to magnify them.
Attachments
carbon1.jpg (1K views, 647.00 KB)
carbon2.jpg (830 views, 847.00 KB)
carbon3.jpg (952 views, 716.00 KB)
carbon4.jpg (802 views, 645.00 KB)
Replies
carboncactus
carboncactus
Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)
Group: Forum Members
Posts: 243, Visits: 1K
Did you still just whack it straight in the preheated oven?
Did you mix and match pumps and gauges to eliminate any lemons?

This isn't the issue, but you're working with OOA so it's useful:You could also try not using any breather. I didnt use any breather in the BMW S1000RR mudguard above.
It's debatable weather breather actually causes bridging and uneven thicknesses in both concave and convex corners. There's a paper published by a McGill University mechanical engineering student with evidence that breather causes voids in OOA laminates. Also, the bag you are using is extremely stretchy. That, along with the cushioning effect of the breather might be the reason even a full vacuum can't apply enough pressure.

http://www.talkcomposites.com/Uploads/Images/db628ad5-e0e7-47b9-873a-3d84.png
nebraskatrevor
nebraskatrevor
Forum Guru (73 reputation)Forum Guru (73 reputation)Forum Guru (73 reputation)Forum Guru (73 reputation)Forum Guru (73 reputation)Forum Guru (73 reputation)Forum Guru (73 reputation)Forum Guru (73 reputation)Forum Guru (73 reputation)
Group: Forum Members
Posts: 7, Visits: 42
I did mess aouund with pumps and gauges and the results I achieved were with the new pump and new gauge which  performed the best.  What you are saying about the breather and bag is very interesting.  I do have some rigid bagging material and sinceI am just doing amflat shape on glass I think I will try it alonged with a slower progressive cure like you have described.  I did do some slight ramping of the last cure but I started with a cool oven and set it to about 90 deg c and just let it go from cold.  Then after about 2 hrs i raised the temp to about 120 deg c and gave it another half hour before letting it cool back to room temp in an open oven before demolding.  Again thanks for all of your help.
carboncactus
carboncactus
Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)
Group: Forum Members
Posts: 243, Visits: 1K
I'll let someone from EC tell me otherwise, but I think you'll find the surface layer cures between 65 and 120.
16 hours at 65 then for every 10 degrees you increase, cure time is halved (roughly). So 8 hours at 75, 4 hours at 95, 2 hours at 105 and 1 hour at 115/120. 
I ramp from ambient to 65, hold for 3 hours then ramp to 90 for 3 hours, let it cool down by itself then demould. Ramps are done at 1-2 degrees per minute, so it should take 20 minutes to get from 65 to 90.

The reason they ask to cure at 100 is because the backing layers cure at those temperatures. Are you using EC backing prepreg? I may be wrong, but its only what I can guess from my experience with prepregs, and I've used a fair share of them.

http://www.talkcomposites.com/Uploads/Images/db628ad5-e0e7-47b9-873a-3d84.png
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
nebraskatrevor - 12 Years Ago
carboncactus - 12 Years Ago
nebraskatrevor - 12 Years Ago
carboncactus - 12 Years Ago
nebraskatrevor - 12 Years Ago
carboncactus - 12 Years Ago
nebraskatrevor - 12 Years Ago
fgayford - 12 Years Ago
carboncactus - 12 Years Ago
nebraskatrevor - 12 Years Ago
carboncactus - 12 Years Ago
nebraskatrevor - 12 Years Ago
carboncactus - 12 Years Ago
Warren (Staff) - 12 Years Ago
morepower - 12 Years Ago
carboncactus - 12 Years Ago
fgayford - 12 Years Ago
morepower - 12 Years Ago
fgayford - 12 Years Ago
nebraskatrevor - 12 Years Ago
matthieutje65 - 12 Years Ago
carboncactus - 12 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search