I keep coming across the same problem.

In the final stage of flatting and polishing minute white speckles appear in the epoxy. 

My process, 1 st coat , coating epoxy , 8 > 10 hr cure @ 20*

hand 120 dry sand , brush off dust , vacume.

2nd coat , coating epoxy 8 > 10 hrs cure @ 20*

hand sand wet - 320 > 600 > 1200 > 1500 > 2000

everything looks good at this stage even flat finish no blemishes really, just needs buffing up...

so 

machine polish - ( cheap electric car plisher ) onto wet surface -  farecla standard compound G 3 ( SPECKS APPEAR  Wink> farecla ploshiing compound G10 ( SPECKS REMAIN )

it does not always happen but it doeas happen a lot 

any ideas

Ben
neilb
neilb
Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)
Group: Forum Members
Posts: 107, Visits: 504
I would say that the compound is filling in minute holes in the surface, that is unless these white spots wipe off with your finger?
fgayford
fgayford
Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)
Group: Forum Members
Posts: 433, Visits: 1.2K
neilb (04/05/2013)
I would say that the compound is filling in minute holes in the surface, that is unless these white spots wipe off with your finger?


I agree it is probably pin holes. What I have heard some do is to wash out the pinholes with alcohol and use air to blast out the compound residue.

Take some black boot polish and put a few coats on and buff. The black will fill the pinholes and the rest will be removed when polishing.

Yes its a crude way to make things look good but it works.

Fred    
benet
benet
Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)
Group: Forum Members
Posts: 59, Visits: 373
Thanks , i think your both right but im not sure that boot polish will help as im not doing it on carbon but multi colored patterned cloth. 

and i dont have air tools.

I have previously posted with this issue and found another fix by washing with wd40 but its not perfect and i would dearly love the problem to not occur or at least know what im supposed to try to do to stop it from occurring..

I have just gone back to the surface starting at 320 wet and it took a lot of sanding to get rid of the speckles. and then i did the same process but did the compound and finsh by hand to keep a close eye on what was going on. 

Its better but its still not perfect.

The picure is a BEFOR shot

Here is a picture of what i wahttp://www.talkcomposites.com/Uploads/Images/0c605f08-62d2-4065-ad2c-c9a0.jpgs dealing with...
carboncactus
carboncactus
Supreme Being (3K reputation)Supreme Being (3K reputation)Supreme Being (3K reputation)Supreme Being (3K reputation)Supreme Being (3K reputation)Supreme Being (3K reputation)Supreme Being (3K reputation)Supreme Being (3K reputation)Supreme Being (3K reputation)
Group: Forum Members
Posts: 243, Visits: 1K
fgayford (04/05/2013)
neilb (04/05/2013)
I would say that the compound is filling in minute holes in the surface, that is unless these white spots wipe off with your finger?


I agree it is probably pin holes. What I have heard some do is to wash out the pinholes with alcohol and use air to blast out the compound residue.

Take some black boot polish and put a few coats on and buff. The black will fill the pinholes and the rest will be removed when polishing.

Yes its a crude way to make things look good but it works.

Fred    


Boot polish is a wax product, wouldn't that essentially create a repellant film on the top, making a clear coat application a nightmare?

http://www.talkcomposites.com/Uploads/Images/db628ad5-e0e7-47b9-873a-3d84.png
carbonfibreworks
carbonfibreworks
Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)
Group: Forum Members
Posts: 292, Visits: 4.5K
I have had the same problem in the past and this is my cure, rub over the marks with a black white board marker ( non permanent) and then buff with a cloth and spray with a clear coat. Yes I  know it sounds like a bodge but it could salvage the part.

Chris

http://www.talkcomposites.com/Uploads/Images/97e08777-693c-4af1-a27a-86cf.png
neilb
neilb
Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)
Group: Forum Members
Posts: 107, Visits: 504
try to de-gas the epoxy before you apply it. do you have access to any form vacuum equipment?
benet
benet
Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)
Group: Forum Members
Posts: 59, Visits: 373
i dont have access to any vacuum equipment im afraid .. i do stir very slowly and let the resin stand for at least 5 mins before i use it. and i scoop off any collections of bubbles first. also use a heat gun to get rid of bubbles that seems to work very well while im using it  (ie i see tinny bubbles pop) ... Also this is the top coat (brushed on, its synthetic brush and i re-use it , keeping it in acetone between jobs and drying it before use) . its coating resin and im polishing it back to be the top finish. I wonder if what im getting is dust from the surface of the sanded coat below ... i always brush then vacuum ( with a vacuum cleaner) and then brush off with a soft brush, as ive thought it right to steer away from tack cloth of acetone or anything really between coats. Im still a bit miffed ... if anything here sounds or or unnecessary please let me know.

Thanks

Ben 
neilb
neilb
Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)
Group: Forum Members
Posts: 107, Visits: 504
do you heat the resin before mixing or after?

I can recall fred advising another forum user of a technique to remove air bubbles which involves  the resin being pored (when mixed) from a height (around 12-18 inches I think) slowly into another container apparently this causes the air bubbles to pop. worth a try cause its free!

other than that build a degas chamber with some Perspex sheet and tube silicone'd together, make a rubber gasket for the top, piece of Perspex with a small hole in it for the lid and vacuum the air out with a small vacuum cleaner. it just may work!

good luck!
benet
benet
Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)Supreme Being (903 reputation)
Group: Forum Members
Posts: 59, Visits: 373
hi  neilb

 I like the sound of making a de-gassing chamber but not having seen what one does i cant quite picture what your describing ...

could you expand a little ..

ben
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search