I keep coming across the same problem.

In the final stage of flatting and polishing minute white speckles appear in the epoxy. 

My process, 1 st coat , coating epoxy , 8 > 10 hr cure @ 20*

hand 120 dry sand , brush off dust , vacume.

2nd coat , coating epoxy 8 > 10 hrs cure @ 20*

hand sand wet - 320 > 600 > 1200 > 1500 > 2000

everything looks good at this stage even flat finish no blemishes really, just needs buffing up...

so 

machine polish - ( cheap electric car plisher ) onto wet surface -  farecla standard compound G 3 ( SPECKS APPEAR  Wink> farecla ploshiing compound G10 ( SPECKS REMAIN )

it does not always happen but it doeas happen a lot 

any ideas

Ben
Replies
neilb
neilb
Supreme Being (764 reputation)Supreme Being (764 reputation)Supreme Being (764 reputation)Supreme Being (764 reputation)Supreme Being (764 reputation)Supreme Being (764 reputation)Supreme Being (764 reputation)Supreme Being (764 reputation)Supreme Being (764 reputation)
Group: Forum Members
Posts: 107, Visits: 504
I would say that the compound is filling in minute holes in the surface, that is unless these white spots wipe off with your finger?
fgayford
fgayford
Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)
Group: Forum Members
Posts: 433, Visits: 1.2K
neilb (04/05/2013)
I would say that the compound is filling in minute holes in the surface, that is unless these white spots wipe off with your finger?


I agree it is probably pin holes. What I have heard some do is to wash out the pinholes with alcohol and use air to blast out the compound residue.

Take some black boot polish and put a few coats on and buff. The black will fill the pinholes and the rest will be removed when polishing.

Yes its a crude way to make things look good but it works.

Fred    
carboncactus
carboncactus
Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)
Group: Forum Members
Posts: 243, Visits: 1K
fgayford (04/05/2013)
neilb (04/05/2013)
I would say that the compound is filling in minute holes in the surface, that is unless these white spots wipe off with your finger?


I agree it is probably pin holes. What I have heard some do is to wash out the pinholes with alcohol and use air to blast out the compound residue.

Take some black boot polish and put a few coats on and buff. The black will fill the pinholes and the rest will be removed when polishing.

Yes its a crude way to make things look good but it works.

Fred    


Boot polish is a wax product, wouldn't that essentially create a repellant film on the top, making a clear coat application a nightmare?

http://www.talkcomposites.com/Uploads/Images/db628ad5-e0e7-47b9-873a-3d84.png
fgayford
fgayford
Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)
Group: Forum Members
Posts: 433, Visits: 1.2K
Yes it is wax and you would not be able to clear on to that. I was just suggesting it if you are as done as you are going to go. Then the black in the wax would hide the tiny pin holes.

Fred   
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
benet - 12 Years Ago
neilb - 12 Years Ago
fgayford - 12 Years Ago
carboncactus - 12 Years Ago
fgayford - 12 Years Ago
benet - 12 Years Ago
carbonfibreworks - 12 Years Ago
neilb - 12 Years Ago
benet - 12 Years Ago
neilb - 12 Years Ago
benet - 12 Years Ago
neilb - 12 Years Ago
benet - 12 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search