Race bike seat


Author
Message
carbonfibreworks
carbonfibreworks
Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)
Group: Forum Members
Posts: 292, Visits: 4.5K
I have been working on producing carbon parts for a 250 classic race bike, i used infusion and in total used 14 separate pieces of cloth due to the size and complex shape of the hump on the back of the seat. As it for a classic race bike it will have to be painted as no naked carbon is allowed and the pre trimmed weight is 208 grams.







http://www.talkcomposites.com/Uploads/Images/97e08777-693c-4af1-a27a-86cf.png
Edited 12 Years Ago by Bartonphoenix750
wozza
wozza
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 688, Visits: 5.4K
SmileSmile No going back now, the Infusion Bug has bitten.!!!!!!!!!!!!!!! More pleats/bigger bag. That's why you have the dry looking area in the middle of the part.
Because the bag is stretched too tight once the resin is introduced the bag relaxes a little. Its ok in one direction(length ways) but too tight across the part. (from the pics)
 If the gum tape is being "pulled in" rather than just pressed down then the bag is too small or not positioned correctly.

Warren



Carbon Copies Ltd
Edited 12 Years Ago by wozza
carbonfibreworks
carbonfibreworks
Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)
Group: Forum Members
Posts: 292, Visits: 4.5K
wozza (28/04/2013)
SmileSmile No going back now, the Infusion Bug has bitten.!!!!!!!!!!!!!!! More pleats/bigger bag. That's why you have the dry looking area in the middle of the part.
Because the bag is stretched too tight once the resin is introduced the bag relaxes a little. Its ok in one direction(length ways) but too tight across the part. (from the pics)
 If the gum tape is being "pulled in" rather than just pressed down then the bag is too small or not positioned correctly.

Warren

Hi Warren

Yes your correct no going back, i worked hard to ensure no bridging took place so quite pleased with the outcome and yes a slightly bigger bag would help. I did not have room for a silicon connector at the vacuum end so i cut the vac spiral in half and pushed them into the vac pipe.

Chris

http://www.talkcomposites.com/Uploads/Images/97e08777-693c-4af1-a27a-86cf.png
wozza
wozza
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 688, Visits: 5.4K
Ha Ha welcome to the dark side Smile I am averaging 4/5 Infusions a day, 6 days a week at the moment so I have made plenty of mistakes and had plenty of problems to overcome. Having said that I am sure there are still more issues to come.Crazy

Warren

Carbon Copies Ltd
fgayford
fgayford
Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)
Group: Forum Members
Posts: 433, Visits: 1.2K
I have come up with a way of not using connectors at all.

I wind the spiral around the last inch of plastic tube and wrap a bit of masking tape around the joint to hold it. I then cut off the length of spiral tube I need to cover the span. I wrap a 3 inch strip of tacky tape around the the plastic tube and then stick it down so the perimeter of the vacuum bag goes right over top of it. The two tacky tapes seal just fine with a bit of pressing. I get perfect seal every time.  

Fred  
fgayford
fgayford
Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)
Group: Forum Members
Posts: 433, Visits: 1.2K
You did a nice job there. Remember you can never have a bag too big, but you can have one too small.  Pleats will take up any excess and there is no danger of bridging then.

I think I bag different than most people. I learned a trick from John Burns. I lay my bag down on the table flat and then put the tacky tape all the way around the perimeter. I then flip it over and peel back the paper from a corner and stick it down to one corner of the mold. I the do the same with all 4 corners. I now peel off strips of the paper and work my way around the flanges pinching a pleat and then sticking it down and so on all the way around the bag. To put pleats in like most do is such a pain for me that i feel like it requires the skill of a brain surgeon. I can do a bag in minutes this way with confidence. google John Burns vacuum infusion and he does a youtube demo. I will never go back to sticking the tacky tape down first and then fitting the bag, its much too hard this way.

Once again, only my opinon.

Fred 
carbonfibreworks
carbonfibreworks
Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)
Group: Forum Members
Posts: 292, Visits: 4.5K
fgayford (29/04/2013)
You did a nice job there. Remember you can never have a bag too big, but you can have one too small.  Pleats will take up any excess and there is no danger of bridging then.

I think I bag different than most people. I learned a trick from John Burns. I lay my bag down on the table flat and then put the tacky tape all the way around the perimeter. I then flip it over and peel back the paper from a corner and stick it down to one corner of the mold. I the do the same with all 4 corners. I now peel off strips of the paper and work my way around the flanges pinching a pleat and then sticking it down and so on all the way around the bag. To put pleats in like most do is such a pain for me that i feel like it requires the skill of a brain surgeon. I can do a bag in minutes this way with confidence. google John Burns vacuum infusion and he does a youtube demo. I will never go back to sticking the tacky tape down first and then fitting the bag, its much too hard this way.

Once again, only my opinon.

Fred 


Hi Fred

Yes putting in the pleats was a pain, the size and shape of the mould did not help but the time taken was worth while as i had 100% seal first time. I do remember seeing a John Burns video using the method you described and will try that on one of my next jobs, every day is a school day Smile

Chris

http://www.talkcomposites.com/Uploads/Images/97e08777-693c-4af1-a27a-86cf.png
NikCFC
NikCFC
Supreme Being (483 reputation)Supreme Being (483 reputation)Supreme Being (483 reputation)Supreme Being (483 reputation)Supreme Being (483 reputation)Supreme Being (483 reputation)Supreme Being (483 reputation)Supreme Being (483 reputation)Supreme Being (483 reputation)
Group: Forum Members
Posts: 61, Visits: 871
I agree with Fred, it's way easier making the bag and the pleats this way!
alebassa
alebassa
Supreme Being (332 reputation)Supreme Being (332 reputation)Supreme Being (332 reputation)Supreme Being (332 reputation)Supreme Being (332 reputation)Supreme Being (332 reputation)Supreme Being (332 reputation)Supreme Being (332 reputation)Supreme Being (332 reputation)
Group: Forum Members
Posts: 48, Visits: 171
fgayford (29/04/2013)
You did a nice job there. Remember you can never have a bag too big, but you can have one too small.  Pleats will take up any excess and there is no danger of bridging then.

I think I bag different than most people. I learned a trick from John Burns. I lay my bag down on the table flat and then put the tacky tape all the way around the perimeter. I then flip it over and peel back the paper from a corner and stick it down to one corner of the mold. I the do the same with all 4 corners. I now peel off strips of the paper and work my way around the flanges pinching a pleat and then sticking it down and so on all the way around the bag. To put pleats in like most do is such a pain for me that i feel like it requires the skill of a brain surgeon. I can do a bag in minutes this way with confidence. google John Burns vacuum infusion and he does a youtube demo. I will never go back to sticking the tacky tape down first and then fitting the bag, its much too hard this way.

Once again, only my opinon.

Fred 




Thank you, this is really a great idea! It's such a pain to make the pleats, especially if the part is little!!


Alessandro
prsw
prsw
Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)Supreme Being (904 reputation)
Group: Forum Members
Posts: 112, Visits: 1K
Is that UD I see on the side?
Did it infuse good?
I did a self-supporting racebike subframe with lots of UD and didn't infuse because it, I have been told, does not wet out if infused.
(or rather i did infuse it first and then wetlay/bagged more material later.)

Bartonphoenix750 (28/04/2013)





http://motoform.blogspot.se

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search