hello
This is what I would do.
Get a piece of aluminium sheet and bend it to follow the profile from the inside.
Put packing tape over the aluminium to act as a release film.
Bevel back from the broken edge at least one inch and use 80 grit paper to etch the surface.
Now clamp the aluminium plate snug from the inside and wet lay up your epoxy carbon over this.( the plate should extend farther than the missing part you want to make.)
It should be pretty uniform. Put peelply on this to help consolidate the carbon layers.
Once cured the aluminium will peel away cleanly.
Now scuff the inside, overlapping the area behind the bevel you did on the front
Now lay your carbon on the inside as you did the outside, peelply again.
Once cured you can trim down the excess and flat sand a bit.
If you want to go nuts cosmetically you can brush on o smooth layer of epoxy resin only.
Hope this helps